Ruthenium-based ammonia synthesis catalyst and preparation method and application thereof
By preparing calcium oxide/graphite composite materials as support using cyanamide waste residue, the problem of the decrease in activity of ammonia synthesis catalyst under high temperature and high pressure conditions is solved, and a high-efficiency and low-cost ruthenium amino synthesis catalyst is achieved, which improves the activity and dispersion of the catalyst Spend.
Patent Information
- Application Number
- CN202411308407.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The existing ammonia synthesis catalysts have problems such as methanation of carbon support under high temperature and high pressure conditions, low specific surface area of alkaline earth metal oxide support, which is not conducive to metal ruthenium dispersion and excessive hydrogen adsorption, resulting in a decrease in catalyst activity.
Calcium oxide/graphite composite materials are prepared as the catalyst support for ruthenium-based amino synthesis by acid treatment, alkali treatment, ball milling and calcination, thereby improving the dispersion and specific surface area of ruthenium dispersion and specific surface area.
A high-activity and low-cost ruthenium amino synthesis catalyst is achieved, which solves the problems of poor activity and high energy consumption of traditional catalysts under low temperature and low pressure conditions, and increases the added value of cyanamide waste residue.
Smart Images

Figure CN119076040A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a method for preparing a ruthenium-based ammonia synthesis catalyst using cyanamide waste residue as a raw material, and a product and application thereof. Background Art
[0002] Ammonia (NH3) is an important raw material for the production of fertilizers, dyes and explosives. It is also an ideal hydrogen energy carrier. It is a zero-carbon molecule with high hydrogen storage content (17.8wt%), high volume density (121kg H2 / m 3 , 1MPa), and H2 can be liquefied at 8°C and 2.5MPa for storage and transportation.
[0003] The Haber-Bosch process currently used in the industrial ammonia synthesis process is carried out under high temperature and high pressure conditions of 400-500℃ and 10-30MPa, which consumes 1%-2% of the total global energy supply and emits about 670 million tons of carbon dioxide each year. The ammonia synthesis industry has high energy consumption and emits a large amount of greenhouse gases during the reaction process. With the energy crisis and environmental problems becoming increasingly serious, the traditional ammonia synthesis process faces huge challenges. The key to solving the high energy consumption of the traditional ammonia synthesis industry is to improve the efficiency of the catalytic reaction and reduce the reaction temperature and reaction pressure, which requires the development of low-temperature, low-pressure and highly active ammonia synthesis catalysts.
[0004] At present, the main catalyst for ammonia synthesis industry is iron catalyst. For example, the patent specification with publication number CN106799232A discloses a nano-iron-modified iron-based ammonia synthesis catalyst prepared by solid phase reaction at room temperature, and its preparation method and application, which is to uniformly mix the iron-based ammonia synthesis catalyst, the iron precursor and the solid reagent, grind, ball mill or stir, so that the iron precursor and the solid reagent react on the iron-based ammonia synthesis catalyst carrier, and after the reaction, the product is filtered, washed, dried, and heat-treated under air, nitrogen, argon or vacuum conditions to obtain the final nano-iron-modified iron-based ammonia synthesis catalyst, and the nano-iron loading is 0.1-20wt%.
[0005] Compared with iron catalysts, ruthenium catalysts have higher ammonia synthesis activity under low temperature and low pressure conditions, which can greatly reduce the energy consumption of the ammonia synthesis industry and are known as the second-generation ammonia synthesis catalyst. For example, the patent specification with publication number CN114733551A discloses the design, preparation and application of a high-performance Ru-based ammonia synthesis catalyst, which synthesizes a BN carrier, synthesizes a Ru / BN catalyst, and then loads rare earth elements on the Ru / BN catalyst by an equal volume impregnation method, finally obtaining a RuM / BN catalyst.
[0006] Carbon materials represented by activated carbon, carbon nanotubes, and carbon fibers are often used as carriers of ruthenium-based ammonia synthesis catalysts because of their high specific surface area and strong electron transfer capacity. However, under high temperature and high pressure conditions, carbon carriers are prone to react with hydrogen to generate methane under the catalysis of metallic ruthenium, which causes the loss of carbon carriers and ultimately leads to a decrease in catalyst activity and deactivation. Using crystalline carbon materials such as graphite directly as ruthenium-based ammonia synthesis catalyst carriers requires strong oxidation treatment of crystalline carbon materials such as graphite, which has a complex preparation process and a high yield and low cost. In addition, it is difficult to load additives such as alkaline earth metal oxides on crystalline carbon materials such as graphite, and there is a problem of separation of graphite and alkaline earth metal oxides.
[0007] Although alkaline earth metal oxide materials do not have the problem of methanation, they have a low specific surface area, which is not conducive to the dispersion of metallic ruthenium. In addition, the ruthenium catalyst supported by alkaline earth metal oxides has a serious problem of excessive hydrogen adsorption (hydrogen poisoning), which limits its application.
[0008] Therefore, developing a ruthenium-based ammonia synthesis catalyst carrier that can effectively disperse metallic ruthenium and has high stability is crucial for developing a low-temperature, low-pressure and highly active ammonia synthesis catalyst. Summary of the invention
[0009] In view of the above technical problems and the shortcomings in the art, the present invention provides a method for preparing a ruthenium-based ammonia synthesis catalyst using cyanamide waste residue as a raw material, and a product and application thereof, wherein the cyanamide waste residue is a byproduct of the production process of preparing cyanamide using calcium cyanamide as a raw material. The present invention can solve the problems of easy methanation of ammonia synthesis catalyst carbon carrier and low specific surface area of alkaline earth metal oxide carrier.
[0010] In a first aspect, the present invention provides a method for preparing a ruthenium-based ammonia synthesis catalyst using cyanamide waste residue as a raw material, comprising:
[0011] Step 1: treating the cyanamide waste residue with acid and alkali;
[0012] Step 2: ball milling the waste residue after the treatment in step 1, and calcining the ball-milled material under an inert atmosphere;
[0013] Step 3: mixing the calcined product of step 2 with a ruthenium source and an additive and subjecting the mixture to ball milling to obtain a ruthenium-based ammonia synthesis catalyst; the mass content of calcium oxide in the ruthenium-based ammonia synthesis catalyst is 60%-80%.
[0014] In step 1, the cyanamide waste residue contains calcium carbonate, nitrogen-doped graphite carbon and calcium fluoride. Further, in the cyanamide waste residue, the content of calcium carbonate can be 70wt%-90wt%, the content of nitrogen-doped graphite carbon can be 5wt%-10wt%, and the content of calcium fluoride can be 0.5wt%-2wt%. Due to the characteristics of the cyanamide waste residue itself, the calcium carbonate in the cyanamide waste residue is coated with nitrogen-doped graphite carbon, and the particle size can be 100-1000μm.
[0015] The present invention prepares the calcium oxide / graphite composite material by acid etching treatment and alkali etching treatment, high-energy ball milling and roasting. The calcium oxide / graphite composite material has the following characteristics: specific surface area of 40-100m 2 / g, wherein the calcium oxide is coated with oxygen-deficient, nitrogen-doped graphite carbon. The present invention further uses the calcium oxide / graphite composite material as a carrier to prepare a ruthenium-based ammonia synthesis catalyst. Compared with catalysts with traditional calcium oxide carriers, the ruthenium-based ammonia synthesis catalyst has a high specific surface area (up to 40-100m 2 / g or more), high ruthenium dispersion and high activity.
[0016] In step 1, the cyanamide waste residue can be subjected to acid treatment and alkali treatment in sequence.
[0017] The acid treatment in the present invention, on the one hand, is to regulate the content of calcium carbonate in the material by reacting the acid with the calcium carbonate in the nitrogen-doped graphite carbon coating structure; on the other hand, it is to increase the content of oxygen-containing functional groups in the cyanamide waste residue; and in addition, the interaction between the nitrogen-doped graphite carbon and the calcium carbonate can be regulated by reconstructing the calcium species on the surface of the calcium carbonate in the confined space of the nitrogen-doped graphite carbon coating structure; finally, after ball milling and heat treatment, the dispersion of calcium oxide, subsequent additives and ruthenium in the calcium oxide / graphite composite material is improved.
[0018] Preferably, the mass content of calcium oxide in the ruthenium-based ammonia synthesis catalyst is 60%-80%, and the ruthenium-based ammonia synthesis catalyst at this content has excellent catalytic activity. The acid treatment operation in step 1 can be performed according to this goal.
[0019] In step 1, the acid used in the acid treatment may include at least one of nitric acid, hydrochloric acid and sulfuric acid, preferably nitric acid, which can further improve the catalyst activity.
[0020] In step 1, the concentration of the acid used in the acid treatment may be 0.5-3 mol / L, such as 0.5 mol / L, 1.5 mol / L, etc.
[0021] In step 1, the ratio of the mass of the cyanamide waste residue to the volume of the acid solution used for the acid treatment can be 1-10g:10mL.
[0022] In step 1, the acid treatment time may be 0.5-2 hours, such as 0.5 hours, 1 hour, 1.5 hours, etc. In some embodiments, it is preferably 0.5 hours. Excessive acid treatment may reduce the activity of the catalyst.
[0023] In step 1, the temperature of the acid treatment may be 30-100°C, such as 60°C, 80°C, etc.
[0024] The alkali treatment in the present invention is to remove alkali-soluble impurities, such as silicon dioxide, etc., by reacting alkali with alkali-soluble compounds to improve the catalyst activity.
[0025] In step 1, the alkali used in the alkali treatment may include at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, and cesium hydroxide, preferably sodium hydroxide, which can further improve the catalyst activity.
[0026] In step 1, the concentration of the alkali used in the alkali treatment may be 0.01-5 mol / L, such as 0.1 mol / L, 0.5 mol / L, etc.
[0027] In step 1, the ratio of the mass of the cyanamide waste residue to the volume of the alkaline solution used for the alkaline treatment can be 1-10g:10mL.
[0028] In step 1, the alkali treatment time may be 0.5-2 hours, such as 0.5 hours, 1 hour, etc.
[0029] In step 1, the temperature of the alkali treatment may be 30-100°C, such as 50°C, 60°C, etc.
[0030] In step 2, the ball milling treatment time can be 0.5-6h.
[0031] In step 2, the rotation speed of the ball milling process may be 200-400 rpm.
[0032] In step 2, the ball-to-material ratio of the ball milling process may be 20-40:1.
[0033] In step 2, the atmosphere of the ball milling treatment may be at least one of a rare gas (such as argon) atmosphere, a nitrogen atmosphere, and a hydrogen atmosphere.
[0034] In step 2, the inert atmosphere may be at least one of a rare gas (such as argon) atmosphere and a nitrogen atmosphere.
[0035] In step 2, the calcination temperature may be 500-800°C, such as 600°C, 700°C, etc., preferably 500-600°C, which can further improve the catalyst activity.
[0036] In step 2, the calcination time may be 1-3 hours.
[0037] The product after calcination in step 2 is a calcium oxide / graphite composite material with a specific surface area of 40-100m 2 / g, in which calcium oxide is coated by oxygen-deficient, nitrogen-doped graphitic carbon.
[0038] In step 3, the mass ratio of ruthenium in the ruthenium source to the product calcined in step 2 can be 1-5:100.
[0039] In step 3, the mass ratio of the auxiliary agent to the ruthenium source may be 1-3:1.
[0040] In step 3, the ruthenium source may include at least one of ruthenium nitrosyl nitrate, ruthenium chloride, triruthenium dodecacarbonyl, and ruthenium acetylacetonate.
[0041] In step 3, the auxiliary agent may include at least one of potassium nitrate, barium nitrate, lithium nitrate, cesium nitrate, cerium nitrate, lanthanum nitrate, and yttrium nitrate.
[0042] In step 3, the ball milling time may be 0.5-6 h, such as 1 h.
[0043] In step 3, the rotation speed of the ball mill can be 50-100 rpm.
[0044] In step 3, the ball-to-material ratio of the ball milling can be 5-15:1.
[0045] In step 3, the ball milling atmosphere is at least one of a rare gas (such as argon) atmosphere, a nitrogen atmosphere, and a hydrogen atmosphere.
[0046] The method of the invention is simple and easy to operate, and not only prepares a high-efficiency catalyst for synthesizing ammonia at a relatively low production cost, but also effectively solves the problem that the alkaline earth metal oxide material has a low specific surface area and is not conducive to the dispersion of metal ruthenium, thereby increasing the added value of cyanamide waste residue.
[0047] In a second aspect, the present invention provides a ruthenium-based ammonia synthesis catalyst prepared by the method described in the first aspect.
[0048] In a third aspect, the present invention provides use of the ruthenium-based ammonia synthesis catalyst described in the first aspect in catalytic synthesis of ammonia.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] 1. The present invention utilizes the nitrogen-doped graphite carbon coated calcium carbonate structure in the cyanamide waste residue, and prepares the nitrogen-doped graphite carbon coated calcium oxide composite material (specific surface area to 40-100m 2 / g), which solves the problem that calcium oxide alone as an ammonia synthesis catalyst carrier has poor activity, low specific surface area and low dispersion of metallic ruthenium.
[0051] 2. The nitrogen-doped graphite carbon coated calcium oxide and structure prepared by the present invention, graphite and calcium oxide are uniformly coated and mixed at the nanometer level, which solves the problem of the inertness of the surface of the graphite material, the large density difference with the alkaline earth metal oxide, and the easy separation of graphite and alkaline earth metal oxide.
[0052] 3. The activity of the ruthenium-based ammonia synthesis catalyst prepared by the present invention is much higher than that of the catalyst prepared by directly mixing graphitized carbon and calcium carbonate and using calcium oxide material prepared from pure calcium carbonate as a carrier. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 It is the X-ray diffraction (XRD) diagram of cyanamide waste residue (FZ) and FZ-1-BM6 in Example 1.
[0054] Figure 2 The ammonia synthesis catalyst of Example 1 and Comparative Examples 1-3 was heated at 400°C for 10000 h. -1 Space velocity, outlet ammonia concentration and reaction rate (r m )Result graph. DETAILED DESCRIPTION
[0055] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0056] In the cyanamide waste residue used in the specific embodiment, the content of calcium carbonate is 70wt%-90wt%, the content of nitrogen-doped graphite carbon is 5wt%-10wt%, and the content of calcium fluoride is 0.5wt%-2wt%. The calcium carbonate in the cyanamide waste residue (still present as calcium carbonate after acid-base treatment, which can be proved by XRD) is coated by nitrogen-doped graphite carbon and has a particle size of 100-1000μm.
[0057] Example 1
[0058] Take cyanamide waste residue (XRD results as Figure 1 The method comprises the following steps:
[0059] 1) Acid and alkali treatment of cyanamide waste residue: First, 80 g of cyanamide waste residue was dissolved in 800 mL of 1.5 mol·L -1 The product was treated with acid in nitric acid solution and refluxed in a water bath at 80°C for 0.5 h. Then, the product was treated with alkali, i.e., 10 g of the product after acid treatment was weighed and dissolved in 100 mL of 0.5 mol·L -1 The mixture was refluxed in a sodium hydroxide solution at 60°C in a water bath for 1 hour. The final product was labeled as FZ-1.
[0060] 2) High-energy grinding treatment of FZ-1
[0061] Weigh 4 g of the FZ-1 sample from step 1), add stainless steel ball milling beads with a ball-to-material ratio of 20:1, fill with Ar gas, and mill for 6 h at a ball milling speed of 400 rpm. Then calcine at 600 °C for 2 h in an Ar atmosphere. The final product is a carrier, labeled FZ-1-BM6, and the XRD results are as follows: Figure 1 shown.
[0062] 3) Preparation of ruthenium-based ammonia synthesis catalyst
[0063] Weigh 3 g of the FZ-1-BM6 sample in step 2, then add 0.12 g of triruthenium dodecacarbonyl, 0.15 g of potassium nitrate, and 0.12 g of barium nitrate, mix and ball mill for 1 hour at a ball milling speed of 100 rpm, a ball-to-material ratio of 10:1, and an Ar atmosphere to obtain a ruthenium-based ammonia synthesis catalyst having a calcium oxide content of 60 wt%.
[0064] Example 2
[0065] The only difference from Example 1 is that there is no acid treatment in step 1), and 10 g of cyanamide waste residue is directly treated with alkali, and the rest are the same. The calcium oxide content in the obtained catalyst is 90wt%.
[0066] Example 3
[0067] The only difference from Example 1 is that in step 1), the concentration of the nitric acid solution is changed to 0.5 mol·L -1 , the rest being the same, the calcium oxide content in the obtained catalyst is 80wt%.
[0068] Example 4
[0069] The only difference from Example 1 is that the acid treatment temperature in step 1) is changed to 60° C., and the rest is the same. The calcium oxide content in the obtained catalyst is 75 wt %.
[0070] Example 5
[0071] The only difference from Example 1 is that in step 1), nitric acid is replaced by hydrochloric acid of equimolar concentration, and the rest is the same.
[0072] Example 6
[0073] The only difference from Example 1 is that the acid treatment time in step 1) is changed to 1 hour, and the rest is the same. The calcium oxide content in the obtained catalyst is 10 wt%.
[0074] Example 7
[0075] The only difference from Example 1 is that in step 1), the concentration of the sodium hydroxide solution is changed to 0.1 mol·L -1, and the rest are the same.
[0076] Example 8
[0077] The only difference from Example 1 is that the alkali treatment temperature in step 1) is changed to 50° C., and the rest is the same.
[0078] Example 9
[0079] The only difference from Example 1 is that the alkali treatment time in step 1) is changed to 0.5 h, and the rest is the same.
[0080] Example 10
[0081] The only difference from Example 1 is that in step 1), the sodium hydroxide solution is replaced with potassium hydroxide of equimolar concentration, and the rest is the same.
[0082] Embodiment 11
[0083] The only difference from Example 1 is that in step 2), the calcination temperature after ball milling is changed to 700° C., and the rest are the same.
[0084] Example 12
[0085] The only difference from Example 1 is that in step 3), triruthenium dodecacarbonyl is replaced by ruthenium nitrosyl nitrate in an equimolar amount, and the rest is the same.
[0086] Example 13
[0087] The only difference from Example 1 is that in step 3), barium nitrate is replaced by cerium nitrate of equal mass, and the rest is the same.
[0088] Comparative Example 1
[0089] The method uses cyanamide waste residue as raw material to prepare a ruthenium-based ammonia synthesis catalyst, comprising:
[0090] Weigh 3 g of untreated cyanamide waste residue sample, and then calcine it at 600°C for 2 h in an Ar atmosphere as a carrier, then add 0.12 g of triruthenium dodecacarbonyl, 0.15 g of potassium nitrate, and 0.12 g of barium nitrate, mix and ball mill for 1 h, with a ball-to-material ratio of 10:1, the ball milling atmosphere is Ar, and the ball milling speed is 100 rpm to obtain a ruthenium-based ammonia synthesis catalyst.
[0091] Comparative Example 2
[0092] A ruthenium-based ammonia synthesis catalyst is prepared by using a mixture of graphite carbon and calcium carbonate as raw materials, comprising:
[0093] Weigh 1.8 g of calcium carbonate and 1.2 g of graphite, put them into a ball mill at 500 rpm for 6 h, and then calcine them at 600 ° C for 2 h in an Ar atmosphere to obtain a carrier, and then add 0.12 g of triruthenium dodecacarbonyl, 0.15 g of potassium nitrate, and 0.12 g of barium nitrate, mix and ball mill for 1 h. The ball milling speed is 100 rpm, the ball-to-material ratio is 10:1, and the ball milling atmosphere is Ar to obtain a ruthenium-based ammonia synthesis catalyst.
[0094] Comparative Example 3
[0095] A ruthenium-based ammonia synthesis catalyst is prepared using calcium carbonate as a raw material, comprising:
[0096] Weigh 3 g of calcium carbonate and calcine it at 600°C for 2 h in an Ar atmosphere as a carrier. Then add 0.12 g of triruthenium dodecacarbonyl, 0.15 g of potassium nitrate and 0.12 g of barium nitrate and mix them for ball milling for 1 h. The ball milling speed is 100 rpm, the ball-to-material ratio is 10:1, and the ball milling atmosphere is Ar to obtain a ruthenium-based ammonia synthesis catalyst.
[0097] The specific surface area, pore volume and pore diameter of the carriers obtained in Examples 1-13 and Comparative Examples 1-3 are shown in Table 1.
[0098] Table 1
[0099] <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Pore volume (cm 3 / g)]]> Example 1 54 0.5 Example 2 54 0.4 Example 3 51 0.3 Example 4 52 0.3 Example 5 50 0.5 Example 6 50 0.3 Example 7 49 0.3 Example 8 46 0.3 Example 9 45 0.2 Example 10 40 0.2 Embodiment 11 45 0.4 Example 12 54 0.5 Example 13 54 0.5 Comparative Example 1 22 0.5 Comparative Example 2 55 0.2 Comparative Example 3 8 0.3
[0100] In order to test the catalytic activity of the catalyst prepared by the present invention, 2 mL of the ammonia synthesis catalyst obtained in Examples 1-13 and Comparative Examples 1-3 were placed in the isothermal zone of the fixed bed reaction tube, and a mixed gas with a molar ratio of H2:N2 of 3:1 was introduced. After the reduction procedure, the reaction mixture was heated to 375°C and 400°C at a space velocity of 10000 h / min. -1 The catalyst activity was evaluated at a pressure of 5 MPa. The results are shown in Table 2. In Table 2, “-” means that no ammonia was detected.
[0101] Table 2
[0102]
[0103] Figure 2 The ammonia synthesis catalysts of Example 1 and Comparative Examples 1-3 were shown to be effective at 400°C and 10000 h. -1 Space velocity, outlet ammonia concentration and reaction rate (r m )result.
[0104] By comparing Example 1 (calcium oxide content of 60wt%), Example 2 (calcium oxide content of 90wt%), Example 3 (calcium oxide content of 80wt%), Example 4 (calcium oxide content of 75wt%), and Example 6 (calcium oxide content of 10wt%), it can be concluded that the catalyst activity in the cyanamide waste residue and the calcium oxide content present a "volcano-type" curve relationship. When the calcium oxide content is too high, the active sites of the catalyst may be covered, resulting in a decrease in the catalyst activity. When the calcium oxide content is too low, the interaction between the active components of the catalyst and the calcium oxide may be weakened, thereby reducing the catalyst activity.
[0105] By comparing Example 1 and Example 5, it can be concluded that after the nitric acid in the acid treatment step is replaced by hydrochloric acid, the catalyst activity at 400°C is reduced from 3.49% to 1.73%. The possible reason is that the chloride ions in the hydrochloric acid will reduce the electron cloud density of the active components and thus reduce the catalyst activity.
[0106] Example 7, Example 8, Example 9 and Example 10 respectively investigated the effects of alkali concentration, alkali treatment temperature, alkali treatment time and alkali type on the catalyst activity. -1 Reduced to 0.1 mol·L -1 , the alkali treatment temperature was reduced from 60°C to 50°C, the alkali treatment time was reduced from 1h to 0.5h, and the alkali type was changed from sodium hydroxide to potassium hydroxide, all of which may lead to excessive impurity SiO2 content and reduce catalyst activity.
[0107] Example 11 investigated the effect of calcination temperature on the catalyst activity after ball milling of cyanamide waste residue. When the calcination temperature was increased from 600°C to 700°C, the particle size of calcium oxide increased, resulting in a decrease in catalyst activity.
[0108] Example 12 investigated the effect of the ruthenium source on the catalyst activity. When the ruthenium source was changed from triruthenium dodecacarbonyl to ruthenium nitrosyl nitrate, there was no effect on the catalyst activity.
[0109] Example 13 investigated the effect of the additive on the catalyst activity. When the additive was changed from barium nitrate to cerium nitrate, there was no effect on the catalyst activity.
[0110] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A method for preparing a ruthenium-based ammonia synthesis catalyst using cyanamide waste residue as raw material, characterized in that: include: Step 1: treating the cyanamide waste residue with acid and alkali; Step 2: ball milling the waste residue after the treatment in step 1, and calcining the ball-milled material under an inert atmosphere; Step 3: mixing the calcined product of step 2 with a ruthenium source and an additive and subjecting the mixture to ball milling to obtain a ruthenium-based ammonia synthesis catalyst; the mass content of calcium oxide in the ruthenium-based ammonia synthesis catalyst is 60%-80%.
2. The method according to claim 1, characterized in that In step 1: The cyanamide waste residue contains calcium carbonate, nitrogen-doped graphite carbon and calcium fluoride; In the cyanamide waste residue, the content of calcium carbonate is 70wt%-90wt%, the content of nitrogen-doped graphite carbon is 5wt%-10wt%, and the content of calcium fluoride is 0.5wt%-2wt%; The calcium carbonate in the cyanamide waste residue is coated with nitrogen-doped graphite carbon and has a particle size of 100-1000 μm.
3. The method according to claim 1, characterized in that In step 1: The acid used in the acid treatment includes at least one of nitric acid, hydrochloric acid and sulfuric acid; The acid concentration used in the acid treatment is 0.5-3 mol / L; The acid treatment time is 0.5-2 hours; The ratio of the mass of the cyanamide waste residue to the volume of the acid solution used for the acid treatment is 1-10g:10mL; The temperature of the acid treatment is 30-100°C.
4. The method according to claim 1, characterized in that: In step 1: The alkali used in the alkali treatment includes at least one of sodium hydroxide, potassium hydroxide, lithium hydroxide, and cesium hydroxide; The concentration of the alkali used in the alkali treatment is 0.01-5 mol / L; The alkali treatment time is 0.5-2 hours; The ratio of the mass of the cyanamide waste residue to the volume of the alkaline solution used for the alkaline treatment is 1-10g:10mL; The temperature of the alkali treatment is 30-100°C.
5. The method according to claim 1, characterized in that: In step 2: The ball milling time is 0.5-6h; The rotation speed of the ball milling process is 200-400 rpm; The ball-to-material ratio of the ball milling process is 20-40:1; The ball milling treatment is performed in an atmosphere selected from at least one of a rare gas atmosphere, a nitrogen atmosphere, and a hydrogen atmosphere.
6. The method according to claim 1, characterized in that In step 2: The inert atmosphere is at least one of a rare gas atmosphere and a nitrogen atmosphere; The calcination temperature is 500-800°C; The calcination time is 1-3 hours.
7. The method according to claim 1, characterized in that In step 3: The mass ratio of ruthenium in the ruthenium source to the product after calcination in step 2 is 1-5:100; The mass ratio of the auxiliary agent to the ruthenium source is 1-3:1; The ruthenium source includes at least one of ruthenium nitrosyl nitrate, ruthenium chloride, triruthenium dodecacarbonyl, and ruthenium acetylacetonate; The auxiliary agent includes at least one of potassium nitrate, barium nitrate, lithium nitrate, cesium nitrate, cerium nitrate, lanthanum nitrate and yttrium nitrate.
8. The method according to claim 1, characterized in that In step 3: The ball milling time is 0.5-6h; The rotation speed of the ball mill is 50-100 rpm; The ball-to-material ratio of the ball mill is 5-15:1; The ball milling atmosphere is at least one of a rare gas atmosphere, a nitrogen atmosphere, and a hydrogen atmosphere.
9. The ruthenium-based ammonia synthesis catalyst prepared by the method according to any one of claims 1 to 8, characterized in that: The mass content of calcium oxide in the ruthenium-based ammonia synthesis catalyst is 60%-80%.
10. Use of the ruthenium-based ammonia synthesis catalyst according to claim 9 in catalytic synthesis of ammonia.
Citation Information
Patent Citations
Nano-iron-modified iron-based ammonia synthesis catalyst prepared by solid-phase reaction at room temperature, and preparation method and application thereof
CN106799232A
High-performance Ru-based synthetic ammonia catalyst as well as preparation method and application thereof
CN114733551A
Method for constructing energy-saving and emission-reduction industrial cluster and radically treating melamine-polluted food
CN102796054A
Method for preparing calcium carbonate whiskers from dicyandiamide waste residues
CN106012012A
Method for preparing lime nitrogen through hydrogen cyanamide production waste residues