Wood-loaded cobalt-nitrogen catalytic material, preparation thereof and application of wood-loaded cobalt-nitrogen catalytic material in purification of organic wastewater

By fixing cobalt species on wood, efficient wood-loaded cobalt nitrogen catalytic material is prepared, which solves the problem of poor stability of reuse of sheet cobalt nitrogen materials, and achieves efficient degradation of organic pollutants and reduces treatment costs. It has good reusable performance and environmental protection characteristics.

CN119076054APending Publication Date: 2024-12-06SOUTH CHINA AGRICULTURAL UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411070284.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing sheet-based cobalt nitrogen materials have poor reuse stability and are difficult to recover in organic pollutant treatment, resulting in high processing costs and low efficiency.

Method used

Using the preparation method of wood-supported cobalt nitrogen (WPCoN) catalytic material, cobalt salt, polyvinylpyrrolidone and nitrogen source react with alkali-treated wood chips under hydrothermal conditions to fix cobalt species on the surface of the wood to form efficient catalytic material , used to activate persulfate treatment of organic pollutants.

Benefits of technology

The stable fixation of cobalt species is achieved, catalytic activity and reusable stability is improved, treatment costs are reduced, the material is easy to recover, and the degradation effect is maintained at 99% in three reuses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076054A_ABST
    Figure CN119076054A_ABST
Patent Text Reader

Abstract

The invention discloses a wood-loaded cobalt-nitrogen catalytic material, preparation thereof and application of the wood-loaded cobalt-nitrogen catalytic material in purification of organic wastewater. The preparation method comprises the following steps: (1) adding cobalt salt, polyvinylpyrrolidone and a nitrogen source into a solvent to obtain a reaction solution; the addition amount of the nitrogen source in the reaction solution is 3-15mM; and (2) putting a wood chip substrate subjected to alkali treatment into the reaction solution in the step (1), and then carrying out hydrothermal reaction at 100-180 DEG C to obtain the wood chip loaded cobalt nitrogen material (WPCoN). The WPCoN material disclosed by the invention can be used for rapidly activating peroxymonosulfate and effectively degrading organic pollutants in a water body. Besides, the stability is extremely good, the removal rate and the removal effect on organic pollutants are basically unchanged in the three-time repeated use process, the degradation rate is still larger than 80% in the five-time use process, the problem that a sheet material is used for activating persulfate to degrade the organic pollutants is solved, and practical significance is achieved in the application of sewage purification.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic wastewater treatment, and in particular relates to a wood-loaded cobalt-nitrogen catalytic material and a preparation method and application thereof in purifying organic wastewater. Background Art

[0002] With the continuous development of industry, handicrafts and medical services, a large amount of organic pollutants flow into water bodies, resulting in increasingly prominent related environmental problems and posing a great threat to the ecological environment. Advanced oxidation processes (AOPs) are currently the most effective and promising methods for treating organic pollutants, mainly by generating free radicals and non-free radicals to attack organic pollutants and mineralize them into water and carbon dioxide. The degradation of pollutants by conventional AOPs (such as the Fenton process) mainly depends on hydroxyl radicals. Hydroxyl radicals are non-selective strong oxidants with a redox potential of 2.8V that can destroy the structure of organic compounds. Recently, persulfate advanced oxidation technology (SR-AOPs) based on sulfate radicals has attracted increasing attention. Compared with hydroxyl radicals, sulfate radicals have the same or even higher redox potential (2.5-3.1V) and can oxidize and decompose organic pollutants more rapidly and non-selectively. In addition, in some cases, sulfate radicals have higher selectivity and longer half-life than hydroxyl radicals. Therefore, sulfate radicals show similar or better ability in degrading emerging pollutants. Transition metals can effectively activate monosulfate and peroxydisulfate to produce sulfate radicals, hydroxyl radicals, superoxide radicals, singlet oxygen and other substances to attack organic pollutants. Among them, cobalt nitrogen materials have the best activation effect on peroxymonosulfate.

[0003] Compared with powdered cobalt nitrogen materials, flake cobalt nitrogen materials are more conducive to recycling and practical use. However, how to ensure the stable growth of cobalt nitrogen species on the surface of the flakes and prevent them from falling off during the reaction process, and improve the repeated use stability of the flake materials are currently a major problem facing the practical application of flake cobalt nitrogen materials. Summary of the invention

[0004] The purpose of the present invention is to provide a wood chip supported cobalt nitrogen (WPCoN) catalytic material and its preparation and application, and a method for improving the stability of the reuse of activated peroxymonosulfate to treat organic pollutants. The method used in the present invention is mild, simple, low in energy consumption, convenient for recycling, high in reuse efficiency, low in processing cost and convenient for transportation.

[0005] In order to achieve the above object, the present invention provides the following technical solutions.

[0006] A method for preparing a wood-supported cobalt-nitrogen catalytic material comprises the following steps:

[0007] (1) adding cobalt salt, polyvinyl pyrrolidone and nitrogen source into a solvent and stirring evenly to obtain a reaction solution; the amount of the nitrogen source added to the reaction solution is 3-15 mM;

[0008] (2) placing the alkali-treated wood chip substrate into the reaction solution of step (1), stirring, and then performing a hydrothermal reaction at 100-180° C. to obtain a wood chip-loaded cobalt nitrogen material (WPCoN).

[0009] Preferably, the nitrogen source is added to the reaction solution in an amount of 9-12 mM.

[0010] Preferably, the temperature of the hydrothermal reaction is 140-180°C.

[0011] Preferably, the cobalt salt is one or more of cobalt nitrate hexahydrate, cobalt acetate, cobalt chloride and cobalt sulfate.

[0012] Preferably, the nitrogen source is one or more of urea, melamine and dicyandiamide.

[0013] Preferably, the solvent is a mixed solvent of water and anhydrous ethanol.

[0014] Preferably, the volume ratio of water to anhydrous ethanol is 1:0.5-1:3, more preferably 1:1.

[0015] Preferably, the concentration of the cobalt salt in the reaction solution is 0.1-5 mM.

[0016] Preferably, the molecular weight of the polyvinyl pyrrolidone is 5800, and the concentration in the reaction solution is 3.45-12.93M.

[0017] Preferably, the hydrothermal reaction time is 10-20 hours, preferably 10-12 hours.

[0018] Preferably, the treatment of the wood chip substrate comprises the following steps: placing the wood chips in an alkali solution with a concentration of 1.5-9wt% and stirring for 1-9 hours; then placing the wood chips in water and continuing to stir, wherein the water is changed every 4 hours until the pH of the solution is less than 9; then drying the treated wood chips to obtain a wood chip substrate; the alkali comprises one or more of sodium hydroxide and potassium hydroxide.

[0019] Preferably, the size of the wood chip is 2*3cm 2 .

[0020] The surface of wood chips has abundant micron-scale pores and is a kind of biomass waste. After treatment, the terminal carboxyl groups on the wood chips can coordinate with cobalt, which can effectively ensure the growth of cobalt species on the surface of the wood chips, thus solving the problem of difficulty in reuse.

[0021] Preferably, after the hydrothermal reaction is completed, the wood chips are taken out, washed with water and alcohol, and then dried to obtain the wood-loaded cobalt-nitrogen catalytic material.

[0022] A wood-supported cobalt-nitrogen catalytic material prepared by any of the preparation methods described above.

[0023] The above-mentioned wood-supported cobalt-nitrogen catalytic material is used to degrade organic pollutants in water, comprising the following steps:

[0024] The wood-loaded cobalt-nitrogen catalytic material is placed in wastewater containing organic pollutants, and after adsorption equilibrium is reached, 1 mL of a sulfate solution is added to the pollutant solution after adsorption equilibrium.

[0025] Preferably, the organic pollutant is one or more of tetracycline hydrochloride, sulfamethoxazole, methylene blue and rhodamine B.

[0026] Preferably, the concentration of the organic pollutants in the wastewater is 5-30 mg / L.

[0027] Preferably, the concentration of the peroxymonosulfate solution is 0.05-0.2M, more preferably 0.1M.

[0028] Preferably, the volume ratio of the peroxymonosulfate solution to wastewater is 0.25:100-2:100, more preferably 1:100.

[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0030] (1) The WPCoN catalytic material prepared by the present invention can effectively fix cobalt on the surface of wood, and has the characteristics of high catalytic activity, high stability, high reusability and easy recycling.

[0031] (2) The WPCoN material prepared by the present invention can effectively activate peroxymonosulfate and efficiently degrade sulfamethoxazole.

[0032] (3) The wood chip-loaded cobalt-nitrogen material of the present invention has good reusability for degrading organic pollutants in water. During three repeated uses, the reaction rate remains basically unchanged and the final degradation degree can reach 99%.

[0033] (4) The preparation method provided by the present invention has the advantages of wide raw material sources, mild reaction conditions, low preparation cost, and green environmental protection. It solves the problem of difficult recovery of catalysts in water bodies and poor reuse performance, and has broad application prospects in the field of environmental remediation. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 WP obtained in Comparative Example 2 900Transmission electron microscopy image of Co3 (A) and corresponding energy spectrum element content image (B).

[0035] Figure 2 WP obtained in Example 1 900 Co3N 12 Transmission electron micrograph (A) and corresponding energy spectrum element content diagram (B).

[0036] Figure 3 This is a degradation performance diagram of the material obtained in Comparative Example 1 after being reused three times.

[0037] Figure 4 This is a degradation performance diagram of the material obtained in Comparative Example 2 after being reused five times.

[0038] Figure 5 This is a graph showing the degradation performance of the material obtained in Example 1 after five repeated uses.

[0039] Figure 6 This is a degradation performance diagram of the material obtained in Example 2 after being reused five times.

[0040] Figure 7 This is a degradation performance diagram of the material obtained in Example 3 after being reused five times.

[0041] Figure 8 This is a degradation performance diagram of the material obtained in Example 4 after being reused five times.

[0042] Fig. 9 This is a degradation performance diagram of the material obtained in Example 5 after being reused five times.

[0043] Fig.10 This is a degradation performance diagram of the material obtained in Example 6 after being reused five times.

[0044] Fig.11 This is a graph showing the degradation performance of the material obtained in Example 7 after being reused five times. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.

[0046] The wood chips used below are processed by the following steps:

[0047] Cut the wood pieces (2*3cm 2 ) was placed in 1.5wt% sodium hydroxide or potassium hydroxide and stirred for 5 hours. The wood chips were then placed in deionized water and stirred for 24 hours, with the water changed every 4 hours, until the pH of the solution was less than 9. The treated wood chips were then placed in an oven and dried at 60°C, which was recorded as the wood chip base.

[0048] The following method for treating wastewater using persulfate advanced oxidation technology comprises the following steps:

[0049] The prepared material (2*3cm 2 ) was placed in 100 mL of a pollutant solution containing 20 mg / L sulfamethoxazole and adsorbed for 30-40 min to reach adsorption equilibrium; then 1 mL of 0.1 M peroxymonosulfate was added to the pollutant solution after adsorption equilibrium.

[0050] Comparative Example 1

[0051] A wood chip loaded nitrogen (WP 900 N 12 ), the specific preparation steps are as follows:

[0052] (1) After 12 mM urea, 900 mg polyvinyl pyrrolidone, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0053] (2) WP obtained in this comparative example 900 N 12 The degradation performance after repeated use for 3 times is as follows Figure 3 As shown, WP 900 N 12 Permonosulfate can be activated to degrade organic pollutants, but the efficiency is low, with the degradation efficiency being only 50% in 60 minutes.

[0054] Comparative Example 2

[0055] A wood chip loaded nitrogen (WP 900 Co3) preparation method, the specific preparation steps are as follows:

[0056] (1) After 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chips are placed in the mixture and stirred for 30 minutes. Then the solution and the wood chip substrate are placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. Then the wood chips are placed in an oven and dried at 50°C for 2 hours.

[0057] (2) WP obtained in this comparative example 900 Co3 transmission electron microscope image and corresponding energy spectrum element content map. Visible WP 900 There are no obvious cobalt particles in Co3, but the element peak corresponding to cobalt can be scanned in the energy spectrum, indicating that cobalt is successfully loaded, but the content is relatively small.

[0058] (3) WP obtained in this comparative example 900 The degradation effect of Co3 after 5 times of reuse is as follows: Figure 4 As shown, during the three uses, the degradation effect gradually worsened and the rate gradually slowed down. The third degradation efficiency was only 73%, and the fifth degradation rate was only 34%.

[0059] Example 1

[0060] A wood chip loaded nitrogen (WP 900 Co3N 12 ), the specific preparation steps are as follows:

[0061] (1) After 12 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0062] (2) WP obtained in this embodiment 900 Co3N 12 Transmission electron microscope image and corresponding energy spectrum element content map. 900 Co3N 12 Obvious cobalt particles can be seen, and the element peak corresponding to cobalt can be scanned in the energy spectrum, indicating that cobalt is successfully loaded and the content is relatively high.

[0063] (3) WP obtained in this embodiment 900 Co3N 12 The degradation performance after repeated use for 5 times is as follows

[0064] Figure 5 As shown in the figure, a similar rate can be maintained during the three repeated uses, and the final degradation rate can still reach 85% at the fifth use.

[0065] Example 2

[0066] A wood chip loaded nitrogen (WP 900 Co3N3) preparation method, the specific preparation steps are as follows:

[0067] (1) After 3 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0068] (2) WP obtained in this embodiment 900 The degradation performance of Co3N3 after five times of reuse is shown in Figure 6 As shown in the figure, the degradation was completely maintained during the two repeated uses, but the performance was greatly reduced after the fifth use.

[0069] Example 3

[0070] A wood chip loaded nitrogen (WP 900 Co3N6) preparation method, the specific preparation steps are as follows:

[0071] (1) After 6 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0072] (2) WP obtained in this embodiment 900 The degradation performance of Co3N6 after five reuses is shown in Figure 7 As shown in the figure, the degradation was completely maintained during the two repeated uses, but the performance was greatly reduced after the fifth use.

[0073] Example 4

[0074] A wood chip loaded nitrogen (WP 900 Co3N9) preparation method, the specific preparation steps are as follows:

[0075] (1) After 9 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0076] (2) WP obtained in this embodiment 900 The degradation performance of Co3N9 after repeated use for 5 times is as follows Figure 8 As shown, the degradation rate can be kept completely during the three times of repeated use, and the degradation rate can still be kept at 74% after the fifth use.

[0077] Example 5

[0078] A wood chip loaded nitrogen (WP 900 Co3N 15), the specific preparation steps are as follows:

[0079] (1) After 15 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 140°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0080] (2) WP obtained in this embodiment 900 Co3N 15 The degradation performance after repeated use for 5 times is as follows Fig. 9 As shown in the figure, the degradation was completely maintained during the two repeated uses, but the performance was greatly reduced after the fifth use.

[0081] Example 6

[0082] A wood chip loaded nitrogen (WP 900 Co3N 12 ), the specific preparation steps are as follows:

[0083] (1) After 12 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 100°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0084] (2) WP obtained in this embodiment 900 Co3N 12 The degradation performance after repeated use for 5 times is as follows

[0085] Fig.10 As shown, the degradation rate can reach more than 80% during the first three reuses, but only about 50% of the degradation effect can be maintained during the fourth and fifth uses.

[0086] Example 7

[0087] A wood chip loaded nitrogen (WP 900 Co3N 12 ), the specific preparation steps are as follows:

[0088] (1) After 12 mM urea, 900 mg polyvinyl pyrrolidone, 3 mM cobalt nitrate hexahydrate, 15 mL water, and 15 mL anhydrous ethanol are mixed evenly, the wood chip substrate is placed in the mixture, and the mixture is stirred for 30 minutes. The solution and wood chips are then placed in a reactor and reacted in an oven at 180°C for 12 hours. After the reaction is completed, the wood chips are taken out and rinsed with water and ethanol three times in turn. The wood chips are then placed in an oven and dried at 50°C for 2 hours.

[0089] (2) WP obtained in this embodiment 900 Co3N 12 The degradation performance after repeated use for 5 times is as follows

[0090] Fig.11 As shown, almost complete degradation can be achieved during the first four reuses, and a degradation rate of more than 80% can be maintained during the fifth use.

Claims

1. A method for preparing a wood-supported cobalt-nitrogen catalytic material, characterized in that: The following steps are involved: (1) adding cobalt salt, polyvinyl pyrrolidone and nitrogen source into a solvent and stirring evenly to obtain a reaction solution; the amount of the nitrogen source added to the reaction solution is 3-15 mM; (2) placing the alkali-treated wood chip substrate into the reaction solution of step (1), stirring, and then performing a hydrothermal reaction at 100-180° C. to obtain a wood chip-loaded cobalt-nitrogen material.

2. The method for preparing a wood-supported cobalt-nitrogen catalytic material according to claim 1, characterized in that: The amount of the nitrogen source added to the reaction solution is 9-12 mM; the temperature of the hydrothermal reaction is 140-180°C.

3. The method for preparing a wood-supported cobalt-nitrogen catalytic material according to claim 1, characterized in that: The cobalt salt is one or more of cobalt nitrate hexahydrate, cobalt acetate, cobalt chloride and cobalt sulfate; the nitrogen source is one or more of urea, melamine and dicyandiamide; the solvent is a mixed solvent of water and anhydrous ethanol; the volume ratio of water to anhydrous ethanol is 1:0.5-1:

3.

4. The method for preparing a wood-supported cobalt-nitrogen catalytic material according to claim 1, characterized in that: The concentration of the cobalt salt in the reaction solution is 0.1-5 mM; the concentration of the polyvinyl pyrrolidone in the reaction solution is 3.45-12.93 M.

5. The method for preparing a wood-supported cobalt-nitrogen catalytic material according to claim 1, characterized in that: The hydrothermal reaction time is 10-20 hours, preferably 10-12 hours.

6. The method for preparing a wood-supported cobalt-nitrogen catalytic material according to claim 1, characterized in that: The treatment of the wood chip substrate comprises the following steps: placing the wood chips in an alkali solution with a concentration of 1.5-9wt% and stirring for 1-9 hours; placing the wood chips in water and continuing to stir, wherein the water is changed every 4 hours until the pH of the solution is less than 9; then drying the treated wood chips to obtain a wood chip substrate; the alkali comprises one or more of sodium hydroxide and potassium hydroxide; After the hydrothermal reaction is completed, the wood chips are taken out, washed with water and alcohol, and then dried to obtain the wood-supported cobalt-nitrogen catalytic material.

7. A wood-supported cobalt-nitrogen catalytic material prepared by the preparation method according to any one of claims 1 to 6.

8. The wood-supported cobalt-nitrogen catalytic material according to claim 7 is used to degrade organic pollutants in water, characterized in that: The following steps are involved: The wood-loaded cobalt-nitrogen catalytic material is placed in wastewater containing organic pollutants, and after adsorption equilibrium is reached, a peroxymonosulfate solution is added to the pollutant solution after adsorption equilibrium.

9. The wood-supported cobalt-nitrogen catalytic material for degrading organic pollutants in water according to claim 8, characterized in that: The organic pollutants are one or more of tetracycline hydrochloride, sulfamethoxazole, methylene blue and rhodamine B; and the concentration of the organic pollutants in the wastewater is 5-30 mg / L.

10. The wood-supported cobalt-nitrogen catalytic material for degrading organic pollutants in water according to claim 8, characterized in that: The concentration of the peroxymonosulfate solution is 0.05-0.2M, and the volume ratio of the peroxymonosulfate solution to the wastewater is 0.25:100-2:100.