Box column welding method
Through the combined process of laser arc composite welding and submerged arc welding, the box column welding process is optimized, and the problems of frequent welding times and large consumption of welding materials in the existing technology are solved, the welding efficiency and quality are improved, and the structural strength is enhanced. Reduced costs.
Patent Information
- Application Number
- CN202411260671.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing box column welding process has problems such as the number of welding times/layers, large welding material consumption, low welding efficiency and welding quality that needs to be improved, mainly due to the unreasonable design of bevels and blunt edges and the improper setting of welding process parameters.
Single-sided welding and double-sided forming is carried out by laser arc composite welding technology. There is no need to open a bevel for box columns with a wall thickness of not more than 16mm. Box columns with a wall thickness of not more than 16mm are left with 15mm blunt edges for laser arc composite welding and base welding. , and fill welding using submerged arc welding process in the bevel area, optimizing welding parameters to reduce unnecessary steps and welding material consumption.
It improves welding efficiency and quality, reduces welding costs, enhances structural strength, and optimizes welding process and parameter settings, reduces welding times and welding material consumption, and improves the overall load-bearing capacity and safety of box columns.
Smart Images

Figure CN119077132A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of welding methods, and particularly to a welding method for box columns. Background Art
[0002] Box columns get their name because their shape resembles a large iron box. They are generally used as beams or columns in steel structures. Specific drawings may vary. Some are like the "#" shape with all four sides protruding, some are like the "□", and there are also semi-closed ones. Therefore, drawings are necessary for the processing of box columns.
[0003] Most of the existing welding processes for box columns use submerged arc welding, that is, a groove is opened at the joint, with a root face of about 4 mm left. A backing plate needs to be attached to the bottom of the weld, and then submerged arc welding is used for backing welding. After welding, root cleaning treatment is required to grind off the oxide scale on the weld surface, and then submerged arc welding in the groove is used for filling welding, and multiple filling welds are required. For example, for a box column with a wall thickness of 20 mm, the weld groove area needs to be filled and welded 3 times (wire diameter 4 mm). Its welding technology is relatively mature. However, the applicant has found that it still has at least one of the following defects: a relatively large number of welding layers / times, a large consumption of welding materials, a relatively low welding efficiency, and the welding quality needs to be improved. Summary of the Invention
[0004] In order to solve at least one of the above technical problems, and to develop a welding process that can effectively improve the welding quality of box columns, and can effectively simplify the welding process, reduce the number of welding times / layers and the consumption of welding materials, and greatly improve the welding processing efficiency of box columns, the present application provides a welding method for box columns.
[0005] The present application provides a welding method for box columns, including the following steps:
[0006] For box columns with a wall thickness not exceeding 16 mm, no groove treatment is required, and a laser-arc hybrid welding process is used for one-time welding to form a single-sided weld with double-sided formation.
[0007] For box columns with a wall thickness exceeding 16 mm, groove treatment is required, with a root face of 15 mm left, and a laser-arc hybrid welding process is used for backing welding, with the 15-mm root face welded in one pass, and submerged arc welding is used for filling welding in the groove area.
[0008] Optionally, for box columns with a wall thickness not exceeding 16 mm, the welding parameters of the laser-arc hybrid welding process are: welding speed 140 - 200 cm / min, laser power 8 - 18 kW, wire feeding speed 8 - 13 m / min, and welding current 240 - 280 A.
[0009] Optionally, for box-type columns with a wall thickness exceeding 16 mm, the welding parameters of the laser arc hybrid welding process are: welding speed 150 cm / min, laser power 18 kW, wire feeding speed 12 m / min, and welding current 280 A.
[0010] Optionally, for box columns with wall thickness exceeding 16 mm, the bevel face angle is 30° and the bevel angle is 60°.
[0011] Optionally, for a box column with a wall thickness exceeding 16 mm, the number of welding layers in the groove area is determined according to the wall thickness of the box column and the submerged arc welding process parameters.
[0012] Further optionally, the groove area is welded by submerged arc welding with a single wire, the diameter of the welding wire is 3.2 to 4 mm, the welding current of the welding wire is 650 to 750 A, the welding voltage of the welding wire is 35 to 40 V, and the welding speed is 0.2 to 0.3 m / min.
[0013] Further optionally, the diameter of the welding wire is 4 mm, the welding current of the welding wire is 700 A, the welding voltage of the welding wire is 37.8 V, and the welding speed is 0.22 m / min.
[0014] Further optionally, for a box column with a wall thickness of 20 mm, the groove area may be filled and welded once.
[0015] Optionally, before laser arc hybrid welding, the upper flange plate, the left web plate, the lower flange plate and the right web plate are assembled and spot welded to form a rectangular frame.
[0016] Further optionally, after the welds formed between the upper flange plate and the left web plate and the right web plate are welded along the length direction of the upper flange plate, the rectangular frame is flipped 180° and the welds formed between the lower flange plate and the left web plate and the right web plate are welded along the length direction of the lower flange plate.
[0017] In summary, the present invention includes at least one of the following beneficial technical effects:
[0018] 1. Improve welding processing efficiency: This application adopts specific welding methods and process parameters for box-type columns with different wall thicknesses, which reduces unnecessary steps in the welding process and improves the overall welding efficiency;
[0019] 2. Ensure welding quality: This application directly adopts the laser arc hybrid welding process or the combination of the laser arc hybrid welding process and the submerged arc welding process according to the wall thickness, which ensures the penetration and density of the weld and reduces the occurrence of defects such as incomplete penetration, slag inclusion and porosity;
[0020] Specific welding parameter settings and welding sequence design further ensure the stability and reliability of welding quality;
[0021] 3. Reduce welding costs: This application reduces welding materials and labor costs by optimizing the welding process and reducing the number of welding times (for example, the groove area of a box-type column with a wall thickness of 20 mm only needs to be filled and welded once);
[0022] 4. Enhanced structural strength: The high-quality welded joints obtained by welding in this application enhance the overall structural strength of the box column and improve its bearing capacity and safety;
[0023] 5. High flexibility: The solution designed in this application can flexibly cope with box columns of different wall thicknesses and has strong applicability and operability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the structure of a box-type column (with a wall thickness of 11 mm) according to Example 1 of the present application;
[0025] Figure 2 This is a schematic diagram of the structure of a box-type column (with a wall thickness of 20 mm) according to Example 2 of the present application;
[0026] Figure 3 for Figure 2 A schematic diagram of the local enlarged structure at point A in the middle;
[0027] Figure 4 This is a picture of the weld of the box column welded in Example 2 of the present application;
[0028] In the figure: 1. upper flange plate; 2. left web plate; 3. lower flange plate; 4. right web plate; 5. groove; 6. blunt edge. DETAILED DESCRIPTION
[0029] The present application is further described in detail below with reference to the accompanying drawings and embodiments.
[0030] Unless otherwise specified, the raw materials used in this application are conventional raw materials in the art and can be purchased on the market. The test methods and detection methods in the following examples are conventional methods unless otherwise specified, and the instruments and apparatus used in the tests can be obtained through commercial channels. The parts not elaborated in this specification belong to the prior art.
[0031] After careful research and analysis, the applicant found that the existing box-type column submerged arc welding process in the background technology has at least one of the defects of more welding layers / times, greater consumption of welding materials, lower welding efficiency and welding quality to be improved, which is mainly caused by unreasonable design of the groove 5 and the blunt edge 6 and improper selection and parameter setting of the welding process. The design of the groove 5 and the blunt edge 6 directly affects the number and efficiency of welding filling. If the angle of the groove 5 is too small or the gap is insufficient, multiple fillings are required to fill the weld, thereby reducing the welding efficiency. The adverse effects caused by the unreasonable design of the blunt edge 6 size are not only reflected in the welding efficiency and welding cost, but also in the welding quality. If the size of the blunt edge 6 is too large, it is difficult for the welding rod or welding wire to reach the bottom of the blunt edge 6 during welding, resulting in the root of the weld not being penetrated, which significantly reduces the mechanical properties of the weld and increases the risk of cracks, thereby affecting the overall structural strength and safety of the box-type column. If the size of the blunt edge 6 is too small, in order to fill the weld groove area, it is necessary to fill the welding materials multiple times, thereby increasing the welding time and workload. In addition, the increase in welding material consumption is bound to increase the welding cost. The selection of specific welding processes and the setting of parameters such as welding current, voltage, and welding speed directly affect not only the quality of the weld, but also the welding efficiency. For example, when using submerged arc welding for base welding, root cleaning is required, which is a time-consuming process and will inevitably extend the welding process cycle. If the parameter settings are unreasonable, such as the welding current is too small, the arc voltage is too high, or the welding speed is too fast, it may lead to insufficient weld filling, requiring multiple fillings, and the weld is not fully melted, not welded, or has defects such as pores and cracks. In addition, the more welding processes there are, the greater the risk of welding quality.
[0032] Based on the above ideas, this application designs a welding method for box-type columns with different wall thicknesses, which is specifically divided into two cases:
[0033] 1. For box columns with wall thickness not exceeding 16 mm:
[0034] No need to open groove 5, directly use laser arc hybrid welding process to achieve single-sided welding and double-sided forming;
[0035] The welding parameters are preferably: welding speed 140-200 cm / min, laser power 8-18 kW, wire feeding speed 8-13 m / min, welding current 240-280 A to ensure welding quality and efficiency;
[0036] 2. For box columns with wall thickness exceeding 16mm:
[0037] A groove 5 needs to be opened (such as by laser cutting), and a 15 mm blunt edge 6 is left. Preferably, the groove surface angle is 30° and the groove angle is 60°, so that the welding gun can penetrate the bottom of the groove area for welding, thereby ensuring the welding quality and reducing the consumption of welding materials;
[0038] The laser arc hybrid welding process is used for base welding to ensure that the 15mm blunt edge 6 is welded in one time; the welding parameters are preferably: welding speed 150cm / min, laser power 18kW, wire feeding speed 12m / min, welding current 280A to ensure welding quality and efficiency;
[0039] The groove area is filled with submerged arc welding, and the number of welding layers is determined according to the wall thickness and submerged arc welding process parameters; preferably, submerged arc welding single wire welding is adopted, the diameter of the welding wire is 3.2-4 mm, the welding current of the welding wire is 650-750 A, the welding voltage of the welding wire is 35-40 V, and the welding speed is 0.2-0.3 m / min to ensure the quality and efficiency of the filling welding.
[0040] The design of this application is the result of extensive research and numerous experiments by the applicant.
[0041] The following are examples of the present application:
[0042] The flange plates and web plates used in the embodiments of the present application are both Q550D steel plates.
[0043] In the welding of the embodiment of the present application, the JQ·H08Mn2MoA welding wire of the Jinqiao brand is selected, and the flux is the JQ·SJ101 welding flux of the Jinqiao brand that matches the welding wire.
[0044] Example 1
[0045] like Figure 1 As shown, the present application takes the welding of a box-type column with a wall thickness of 11 mm as Example 1.
[0046] The box column welding method of this embodiment includes the following steps:
[0047] S1, assembling and spot welding the upper flange plate 1, the left web plate 2, the lower flange plate 3 and the right web plate 4 to form a rectangular frame;
[0048] S2, along the length direction of the upper flange plate 1, respectively performing laser arc hybrid welding on the welds formed between the upper flange plate 1 and the left web plate 2 and between the upper flange plate 1 and the right web plate 4;
[0049] S3, flip the rectangular frame 180 degrees, and perform laser arc hybrid welding on the welds formed between the lower flange plate 3 and the left web plate 2 and between the lower flange plate 3 and the right web plate 4 along the length direction of the lower flange plate 3.
[0050] The welding parameters are: welding speed 180cm / min, laser power 12kW, wire feeding speed 10m / min, and welding current 260A.
[0051] The use of laser arc hybrid welding in this embodiment can not only reduce the total heat input during the welding process, significantly reduce the thermal deformation of the workpiece, improve the appearance of the weld, reduce the energy consumption during the welding process, improve the welding quality and the manufacturing accuracy of the box column, and reduce auxiliary processing procedures such as on-site cutting adjustment, deformation correction, etc., but also does not require beveling of the plate, which can effectively reduce the box column processing procedures. In addition, deep melting hybrid welding can be performed on the weld between the flange plate and the web, and single-sided welding and double-sided forming can be performed, which effectively reduces the number of welding times, reduces welding material consumption, and improves welding efficiency.
[0052] Example 2
[0053] like Figure 2 and Figure 3 As shown, the present application takes the welding of a box-type column with a wall thickness of 20 mm as Example 2.
[0054] The box column welding method of this embodiment includes the following steps:
[0055] S1. Bevel the upper flange plate 1, the left web plate 2, the lower flange plate 3 and the right web plate 4 5, leaving a 15 mm blunt edge 6;
[0056] S2, assembling and spot welding the upper flange plate 1, the left web plate 2, the lower flange plate 3 and the right web plate 4 to form a rectangular frame;
[0057] S3, along the length direction of the upper flange plate 1, the laser arc hybrid welding process is used to perform base welding on the welds formed between the upper flange plate 1 and the left web plate 2, and between the upper flange plate 1 and the right web plate 4, and the 15mm blunt edge is welded in one time;
[0058] S4, along the length direction of the upper flange plate 1, using a submerged arc welding process to perform fill welding on the groove area of the weld between the upper flange plate 1 and the left web plate 2, and between the upper flange plate 1 and the right web plate 4;
[0059] S5, flip the rectangular frame 180 degrees, and use the laser arc hybrid welding process to perform base welding on the welds formed between the lower flange plate 3 and the left web plate 2 and between the lower flange plate 3 and the right web plate 4 along the length direction of the lower flange plate 3, and weld the 15mm blunt edge in one step;
[0060] S6. Along the length direction of the lower flange plate 3, the groove areas of the welds between the lower flange plate 3 and the left web plate 2 and between the lower flange plate 3 and the right web plate 4 are filled with welding by using a submerged arc welding process.
[0061] In S1, the groove surface angle is 30° (the angle between the groove surface and the extension line of the blunt edge), and the groove angle is 60° (the angle between the two groove surfaces, for example, the angle between the groove surface of the upper flange plate 1 and the groove surface of the right web 4); the welding parameters in S3 and S5 are: welding speed 150 cm / min, laser power 18 kW, wire feeding speed 12 m / min, welding current 280 A; the welding parameters in S4 and S6 are: the diameter of the welding wire is 4 mm, the welding current of the welding wire is 700 A, the welding voltage of the welding wire is 37.8 V, the welding speed is 0.22 m / min, and the number of filling welding is 1.
[0062] Compared with the existing box-type column welding process: a groove is opened at the joint, leaving a blunt edge of about 4mm, a pad needs to be attached to the bottom of the weld, and then submerged arc welding is used for base welding. After welding, root cleaning is required (grinding off the oxide scale on the surface of the weld), and then submerged arc welding is performed to fill the groove area, requiring 3 filling weldings (when the wall thickness of the box-type column and the submerged arc welding process parameters are the same as those in Example 2). In this embodiment, the blunt edge 6 is left with 15mm, and the base is welded by laser arc hybrid welding. The 15mm blunt edge 6 is welded and formed in one time, and no root cleaning is required. Submerged arc welding is used in the groove area and only one filling welding is required. Therefore, this embodiment can effectively simplify the welding process, greatly reduce the number of welding times / layers and welding material consumption, and improve the welding processing efficiency of the box-type column.
[0063] In addition, the applicant welded 10 box-type columns in Example 1 and Example 2 respectively, tested their various performances, and took the average value of the performance parameters. The results showed that there were no defects such as pores, slag inclusions, and unfusion inside the welds of the box-type columns after welding in Example 1 and Example 2, and the impact resistance, tensile strength, and bending strength of the welds were better than those of the flange plate and web base materials, and the welding quality was excellent.
[0064] Among them, the defect detection inside the weld shall be measured according to the method recorded in GB / T 11345-2013; the impact absorption energy detection shall be measured according to the method recorded in GB / T 2650-2008; the tensile strength detection shall be measured according to the method recorded in GB / T 2651-2008; the bending strength detection shall be measured according to the method recorded in GB / T 2653-2008.
[0065] pass Figure 4 It can also be seen that the weld quality of the box-type column welding method in Example 2 of the present application is excellent.
[0066] It can be seen that the welding method of the present application can not only effectively reduce the number of welding times and layers, reduce the consumption of welding materials, and improve the welding processing efficiency of the box column, but also has excellent welding quality.
[0067] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A box column welding method, characterized in that: The following steps are involved: For box-type columns with a wall thickness not exceeding 16mm, no groove processing is required. The laser arc hybrid welding process is used for one-time welding and double-sided welding. For box columns with wall thickness exceeding 16mm, groove processing is required, leaving a 15mm blunt edge, and laser arc hybrid welding process is used for base welding. The 15mm blunt edge is welded in one time, and the groove area is filled with submerged arc welding process.
2. A box-type column welding method according to claim 1, characterized in that: For box-type columns with a wall thickness not exceeding 16 mm, the welding parameters of the laser arc hybrid welding process are: welding speed 140-200 cm / min, laser power 8-18 kW, wire feeding speed 8-13 m / min, and welding current 240-280 A.
3. A box-type column welding method according to claim 1, characterized in that: For box-type columns with a wall thickness exceeding 16 mm, the welding parameters of the laser arc hybrid welding process are: welding speed 150 cm / min, laser power 18 kW, wire feeding speed 12 m / min, and welding current 280 A.
4. A box-type column welding method according to claim 1, characterized in that: For box columns with wall thickness exceeding 16 mm, the bevel face angle is 30° and the bevel angle is 60°.
5. A box-type column welding method according to claim 1 or 4, characterized in that: For box columns with a wall thickness exceeding 16 mm, the number of welding layers in the groove area is determined according to the wall thickness of the box column and the submerged arc welding process parameters.
6. A box-type column welding method according to claim 5, characterized in that: The groove area is welded with single-wire submerged arc welding. The diameter of the welding wire is 3.2-4 mm, the welding current is 650-750 A, the welding voltage is 35-40 V, and the welding speed is 0.2-0.3 m / min.
7. A box-type column welding method according to claim 6, characterized in that: The diameter of the welding wire is 4 mm, the welding current of the welding wire is 700 A, the welding voltage of the welding wire is 37.8 V, and the welding speed is 0.22 m / min.
8. A box-type column welding method according to claim 7, characterized in that: For box columns with a wall thickness of 20 mm, the groove area can be filled and welded once.
9. A box-type column welding method according to claim 1, characterized in that: Before laser arc hybrid welding, the upper flange plate, the left web plate, the lower flange plate and the right web plate are assembled and spot welded to form a rectangular frame.
10. A box-type column welding method according to claim 9, characterized in that: After the welds formed between the upper flange plate and the left web plate and the right web plate are welded along the length direction of the upper flange plate, the rectangular frame is flipped 180 degrees, and the welds formed between the lower flange plate and the left web plate and the right web plate are welded along the length direction of the lower flange plate.
Citation Information
Patent Citations
Twin arc submerged arc welding method for thick plate box beam / pillar
CN101780591A
Laser-arc hybrid welding method for Invar die steel
CN105665933A
Welding method of semi-automatic submerged arc welding in full penetration of thick plate
CN114799433A
H-shaped steel composite welding device and welding method
CN118438042A
LASER ARCH HYBRID WELDING PROCESS
DE102020102062A1