All-steel radial tire with bionic structure tread
By using staggered superimposed tread A and tread B in all-steel radial tires, combined with specific material components and preparation methods, the problem of tread anti-treading performance and heat generation cannot be achieved, and the problem of tread anti-treading performance and heat generation are achieved. The balance of good anti-prick performance and low heat generation is achieved, avoiding the risk of thermal stripping of the tread.
Patent Information
- Application Number
- CN202411409940.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
AI Technical Summary
The tread glue of all-steel radial tires has the problem that the anti-thorn performance and heat generation cannot be achieved at the same time, resulting in an increased risk of thermal peeling of the tread.
Using multiple tread glue A and tread glue B that are interlaced and superimposed, the Shore hardness of tread glue A is 2 to 10 degrees higher than tread glue B. Through bionic structural design, specific material components and preparation methods are combined. , ensure that the tires have good anti-puncture performance while maintaining low heat generation.
It effectively solves the problem that the anti-sting performance and low thermal performance of the tread of large-sized all-steel radial tires cannot coexist at the same time, ensuring that the tires have high anti-sting performance while avoiding early tread thermal stripping.
Smart Images

Figure CN119078409A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of all-steel radial tire rubber, in particular to an all-steel radial tire with a bionic structure tread. Background Art
[0002] Since the birth of all-steel radial tires, major tire manufacturers have done countless explorations on the performance of rubber materials. There has always been a contradiction: the hardness of rubber and heat generation cannot be achieved at the same time. Especially in the tread part of large-sized all-steel radial tires, the rubber size is thicker, and rubber is a poor conductor of heat, so the tread rubber must maintain a low heat generation, but this will inevitably lead to a lower hardness of the tread rubber, resulting in poor puncture resistance of the tread. If the hardness of the tread rubber is increased, the heat generation of the tread rubber will increase, which will increase the risk of tread thermal peeling in the early use of large-sized all-steel radial tires. So far, the industry has not had a good solution to this problem.
[0003] Since the current single tire tread rubber has the problem that puncture resistance and heat generation cannot be achieved at the same time, it is necessary to improve this. Summary of the invention
[0004] The technical problem to be solved by the present invention is to solve the problem that a single tread rubber cannot have both puncture resistance and low heat generation. The present invention provides an all-steel radial tire with a bionic structure tread, which solves the problem that a single tread rubber cannot have both puncture resistance and low heat generation, thereby ensuring that the all-steel radial tire has good puncture resistance while also having low heat generation, and will not have the problem of early tread thermal peeling.
[0005] In order to achieve the above technical purpose, the present invention adopts the following technical solution:
[0006] The present invention provides an all-steel radial tire with a bionic structure tread, characterized in that it comprises a plurality of tread rubbers A and B that are staggered and stacked on each other;
[0007] The Shore hardness of the tread rubber A is 2 to 10 degrees higher than that of the tread rubber B.
[0008] The Shore hardness of the tread rubber B is 50 to 70 degrees.
[0009] The number of times the tread rubber A and the tread rubber B are staggered and superimposed is ≥2.
[0010] Preferably, the thickness ratio of the tread rubber A to the tread rubber B is 1:2.
[0011] Preferably, the Shore hardness of the tread rubber A is 8 degrees higher than that of the tread rubber B, the Shore hardness of the tread rubber B is 61 degrees, and the number of times the tread rubber A and the tread rubber B are staggered and superimposed is 3.
[0012] The materials used in the tread rubber A include the following components in parts by weight:
[0013] 10-90 parts of natural rubber, 90-10 parts of styrene-butadiene rubber, 50-90 parts of carbon black, 0-15 parts of white carbon black, 2.5-6 parts of zinc oxide, 1.0-4.5 parts of stearic acid, 1-5 parts of microcrystalline wax, 1.5-5.5 parts of antioxidant, 2-8 parts of softener, 0-3 parts of silane coupling agent, 2.5-5 parts of sulfur, and 1-3.5 parts of accelerator.
[0014] The materials used in the tread rubber B include the following components by weight:
[0015] 100 parts of natural rubber, 10-30 parts of carbon black, 10-25 parts of white carbon black, 3-5 parts of zinc oxide, 2-4 parts of stearic acid, 0.5-2 parts of microcrystalline wax, 1-4 parts of antioxidant, 2-5 parts of silane coupling agent, 1-4 parts of softener, 1.5-5 parts of sulfur, and 1-3 parts of accelerator.
[0016] Preferably, the materials used in the tread rubber A include the following components in parts by weight:
[0017] 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 65 parts of carbon black, 5 parts of white carbon black, 6 parts of zinc oxide, 3 parts of stearic acid, 2 parts of microcrystalline wax, 4 parts of antioxidant, 6 parts of softener, 1 part of silane coupling agent, 3 parts of sulfur, and 2 parts of accelerator.
[0018] The materials used in the tread rubber B include the following components in parts by weight: 100 parts of natural rubber, 25 parts of carbon black, 15 parts of white carbon black, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of microcrystalline wax, 3 parts of antioxidant, 3 parts of silane coupling agent, 2 parts of softener, 2.5 parts of sulfur, and 1.5 parts of accelerator.
[0019] The preparation method of the tread rubber A comprises the following steps:
[0020] Add natural rubber and styrene-butadiene rubber into a meshing internal mixer, mix, add zinc oxide, carbon black, white carbon black, and silane coupling agent, continue mixing, lift the bolt, and then press the bolt and discharge the material to obtain a masterbatch of stage A;
[0021] Adding the first stage A masterbatch, stearic acid, microcrystalline wax and softener into a shearing type internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and discharging the glue to obtain the second stage A masterbatch;
[0022] Add the second-stage masterbatch A into the open mixing mill for mixing, and continue to add sulfur, accelerator and antioxidant, mix and discharge the rubber to obtain tread rubber A.
[0023] The preparation method of the tread rubber B comprises the following steps:
[0024] After adding natural rubber to a meshing internal mixer and mixing, zinc oxide, carbon black, white carbon black and silane coupling agent are added and mixed, the plug is lifted, and then the plug is pressed and the material is discharged to obtain a masterbatch of stage B;
[0025] Adding the first stage B masterbatch, stearic acid, microcrystalline wax and softener into a shearing type internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and discharging the glue to obtain the second stage B masterbatch;
[0026] Add the second-stage masterbatch B into the open mixing mill for mixing, continue to add sulfur, accelerator and antioxidant, mix and discharge the rubber to obtain tread rubber B.
[0027] The all-steel radial tire with a bionic structure tread of the present invention has the following beneficial effects compared with the prior art:
[0028] The all-steel radial tire with a bionic structure tread of the present invention comprises a plurality of tread rubbers A and B that are staggered and stacked with each other, and the Shore hardness of the tread rubber A is 2 to 10 degrees higher than that of the tread rubber B. After years of experiments, the applicant has found that the all-steel radial tire adopts a tread rubber material design with two Shore hardnesses of tree ring bionic structures, which solves the problem that the puncture resistance and low heat generation performance of the tread of a large-size all-steel radial tire cannot coexist at the same time. The invention can ensure that the all-steel radial tire has good puncture resistance and low heat generation at the same time, and will not have the problem of early tread thermal peeling. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 It is a schematic structural diagram of an all-steel radial tire with a bionic structural tread of the present invention;
[0031] Figure 2 for the tree ring structure;
[0032] Figure 3 The relationship between the temperature measurement and tread cutting depth results of the 14.00R25 national standard durability for 47 hours and the hardness difference of the tread rubber A / B in Example 2;
[0033] Figure 4 The relationship between the temperature measurement and tread cutting depth results of the 14.00R25 national standard durability for 47 hours and the number of times n of the tread rubber A / B interlaced superposition;
[0034] Figure 5 It is the relationship between the temperature measurement and tread cutting depth results of the 14.00R25 national standard durability for 47 hours and the ratio of the tread rubber A / B composite thickness in Example 4. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] In order to better understand the present invention but not to limit the scope of the present invention, all the numbers used in this application to express the amount, percentage, and other numerical values should be understood as modified by the word "about" in all cases. Therefore, unless otherwise specified, the numerical parameters listed in the specification and the appended claims are approximate values, which may be changed according to the different ideal properties attempted to be obtained. Each numerical parameter should at least be regarded as obtained based on the reported significant figures and by conventional rounding methods.
[0037] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0038] The embodiment of the present application provides an all-steel radial tire with a bionic structure tread, comprising a plurality of tread rubbers A and B that are staggered and stacked with each other;
[0039] Among them, the Shore hardness of tread rubber A is 2 to 10 degrees higher than that of tread rubber B.
[0040] The all-steel radial tire of the present invention is as follows Figure 1As shown, it includes a plurality of tread rubbers A and B that are staggered and stacked with each other. Specifically, the arrangement of tread rubbers A and B from bottom to top is: tread rubber B / tread rubber A / tread rubber B / tread rubber A / tread rubber B / tread rubber A..., wherein the Shore hardness of tread rubber A is 2 to 10 degrees higher than that of tread rubber B. As is well known, due to the influence of seasonal changes, the growth speed of trees is different, such as Figure 2 As shown in the figure, the annual rings of trees are formed with alternating hard parts 2 and soft parts 1. The annual rings have both high-hardness hard parts and low-hardness soft parts, which makes the tree have a lighter specific gravity and good hardness and mechanical properties. Inspired by this, the applicant has found through years of experiments that the all-steel radial tire adopts a tread rubber material design with two Shore hardness tree annual ring bionic structures, which solves the problem that the puncture resistance and low heat generation performance of the tread of large-size all-steel radial tires cannot coexist at the same time. This invention can ensure that the all-steel radial tire has good puncture resistance and low heat generation at the same time, and will not have the problem of early tread thermal peeling.
[0041] In some embodiments, the Shore hardness of the tread rubber B is 50-70 degrees.
[0042] In some embodiments, the number of times the tread rubber A and the tread rubber B are staggered and overlapped is ≥2.
[0043] In some embodiments, the thickness ratio of tread rubber A to tread rubber B is 1:2.
[0044] In some embodiments, the Shore hardness of tread rubber A is 8 degrees higher than that of tread rubber B, the Shore hardness of tread rubber B is 61 degrees, and the number of times the tread rubber A and the tread rubber B are staggered and superimposed is 3.
[0045] In some embodiments, the materials used in the tread rubber A include the following components in parts by weight:
[0046] 10-90 parts of natural rubber, 90-10 parts of styrene-butadiene rubber, 50-90 parts of carbon black, 0-15 parts of white carbon black, 2.5-6 parts of zinc oxide, 1.0-4.5 parts of stearic acid, 1-5 parts of microcrystalline wax, 1.5-5.5 parts of antioxidant, 2-8 parts of softener, 0-3 parts of silane coupling agent, 2.5-5 parts of sulfur, and 1-3.5 parts of accelerator.
[0047] In some embodiments, the material used for the tread rubber B includes the following components in parts by weight:
[0048] 100 parts of natural rubber, 10-30 parts of carbon black, 10-25 parts of white carbon black, 3-5 parts of zinc oxide, 2-4 parts of stearic acid, 0.5-2 parts of microcrystalline wax, 1-4 parts of antioxidant, 2-5 parts of silane coupling agent, 1-4 parts of softener, 1.5-5 parts of sulfur, and 1-3 parts of accelerator.
[0049] In some embodiments, the natural rubber is natural rubber NR10, the styrene-butadiene rubber is styrene-butadiene rubber SBR1500E, the carbon black is carbon black N234, the white carbon black is white carbon black VN3, the microcrystalline wax is type B microcrystalline wax, the antioxidant includes antioxidant RD and / or antioxidant 4020, the accelerator is accelerator NS, the silane coupling agent is Si69, the softener is environmentally friendly aromatic oil (that is, a commercially available aromatic oil rubber softener), and the sulfur is OT-20 (that is, insoluble sulfur OT-20).
[0050] Preferably, in some embodiments, the material used for the tread rubber A includes the following components in parts by weight:
[0051] 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 65 parts of carbon black, 5 parts of white carbon black, 6 parts of zinc oxide, 3 parts of stearic acid, 2 parts of microcrystalline wax, 4 parts of antioxidant, 6 parts of softener, 1 part of silane coupling agent, 3 parts of sulfur, and 2 parts of accelerator.
[0052] Preferably, in some embodiments, the materials used for the tread rubber B include the following components in parts by weight: 100 parts of natural rubber, 25 parts of carbon black, 15 parts of white carbon black, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of microcrystalline wax, 3 parts of antioxidant, 3 parts of silane coupling agent, 2 parts of softener, 2.5 parts of sulfur, and 1.5 parts of accelerator.
[0053] In some embodiments, the preparation method of tread rubber A comprises the following steps:
[0054] S11, adding natural rubber and styrene-butadiene rubber into an intermeshing internal mixer, mixing, adding zinc oxide, carbon black, white carbon black, and silane coupling agent, and continuing to mix, lifting the bolt, and then pressing the bolt and discharging the material to obtain a masterbatch of stage A;
[0055] S12, adding the first stage A masterbatch, stearic acid, microcrystalline wax, and softener into a shearing type internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and removing the glue to obtain the second stage A masterbatch;
[0056] S13, adding the second-stage masterbatch A into an open mixing mill for mixing, and continuing to add sulfur, accelerator, and antioxidant, mixing, and rubber removal to obtain tread rubber A.
[0057] In some embodiments, the preparation method of the tread rubber B comprises the following steps:
[0058] S21, adding natural rubber to a meshing internal mixer, mixing, adding zinc oxide, carbon black, white carbon black, and silane coupling agent, and continuing to mix, lifting the bolt, and then pressing the bolt and discharging to obtain a masterbatch of stage B;
[0059] S22, adding the first stage B masterbatch, stearic acid, microcrystalline wax, and softener into a shearing type internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and removing the glue to obtain the second stage B masterbatch;
[0060] S23, adding the second-stage masterbatch B into an open mixing mill for mixing, and continuing to add sulfur, accelerator, and antioxidant, mixing, and rubber removal to obtain tread rubber B.
[0061] In some embodiments, the preparation method of tread rubber A comprises the following steps:
[0062] S11, mixing of the first stage A masterbatch: setting the speed of the intermeshing internal mixer to 45 rpm, adding natural rubber and styrene-butadiene rubber into the intermeshing internal mixer and mixing for 45 seconds, then adding zinc oxide, carbon black, white carbon black and silane coupling agent and mixing for 155 seconds, lifting the bolt, and then pressing the bolt for 235 seconds before discharging to obtain the first stage A masterbatch;
[0063] S12, A second stage masterbatch mixing: set the speed of the shearing type internal mixer to 55rpm, add A first stage masterbatch, stearic acid, microcrystalline wax, and softener into the shearing type internal mixer, mix for 75 seconds, lift the plug, hold for 5 seconds, then press the plug and mix for 130 seconds, then lift the plug to the top, change the rotor speed to 35rpm, press the plug and mix for 165 seconds, then discharge the glue to the open mixer, this is A second stage masterbatch;
[0064] S13, set the roller pitch of the mixing mill to 2.5mm, the rotation speed to 10m / s, the cooling roller speed to 8m / s, add the second stage masterbatch and mix for 30 seconds, make a ring for 15 seconds, and swing the mixing for 160 seconds. Then, add sulfur, accelerator and antioxidant. After mixing and swinging for 245 seconds, reverse the cooling roller and break it, and the rubber is discharged to obtain the final mixed rubber, thereby obtaining tread rubber A.
[0065] In some embodiments, the preparation method of the tread rubber B comprises the following steps:
[0066] S21, mixing of the first stage B masterbatch: setting the speed of the intermeshing internal mixer to 45 rpm, adding natural rubber into the intermeshing internal mixer and mixing for 45 seconds, then adding zinc oxide, carbon black, white carbon black and silane coupling agent and mixing for 155 seconds, lifting the plug, and then pressing the plug for 235 seconds before discharging to obtain the first stage B masterbatch;
[0067] S22, B second stage masterbatch mixing: set the speed of the shearing type internal mixer to 55rpm, add B first stage masterbatch, stearic acid, microcrystalline wax and softener into the shearing type internal mixer, mix for 75 seconds, lift the plug, hold for 5 seconds, then press the plug and mix for 130 seconds, then lift the plug to the top, change the rotor speed to 35rpm, press the plug and mix for 165 seconds, then discharge the rubber to the open mixer, this is B second stage masterbatch;
[0068] S23, set the roller distance of the mixing mill to 2.5mm, the rotation speed to 10m / s, the cooling roller speed to 8m / s, add the second stage masterbatch and mix for 30 seconds, make a ring for 15 seconds, and swing the mixing for 160 seconds. Then, add sulfur, accelerator and antioxidant. After mixing and swinging for 245 seconds, reverse the cooling roller and break it. The final mixing is obtained by rubber discharge to obtain tread rubber B.
[0069] The following further describes the all-steel radial tire with a bionic structure tread of the present application with specific embodiments. This section further describes the content of the present invention in conjunction with specific embodiments, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0070] Example 1
[0071] The present application example provides a tread rubber A, the formula of which is shown in Table 1 below.
[0072] Table 1 - Formula of tread rubber A (the data units in Table 1 are all parts by weight)
[0073] raw material AGeneral formula Recipe 1 Recipe 2 Recipe 3 Natural Rubber 90 80 50 30 Styrene Butadiene Rubber 10 20 50 70 Carbon Black 70 65 55 45 White Carbon Black 5 5 10 15 Zinc Oxide 3 6 4 5 Stearic acid 2 3 1.5 3.5 Microcrystalline wax 1.5 2 2.5 3.5 Antioxidant 4 4 5 2.5 Softener 7 6 4 8 Silane coupling agent 1 1 2 3 sulfur 3.5 3 2.5 4.5 Accelerator 2.2 2 3 1.5
[0074] The present application example also provides a tread rubber B, the formula of which is shown in Table 2 below.
[0075] Table 2 - Formula of tread rubber B (the data units in Table 1 are all parts by weight)
[0076] raw material BOrdinary formula Recipe 4 Recipe 5 Recipe 6 Natural Rubber 100 100 100 100 Carbon Black 25 15 25 35 White Carbon Black 25 10 15 25 Zinc Oxide 3 3.5 5 4.5 Stearic acid 4 3 2 2 Microcrystalline wax 4 3 1 2 Antioxidant 4 1 3 2 Softener 5 1 2 4 Silane coupling agent 5 2 3 5 sulfur 3.5 4.5 2.5 1.5 Accelerator 1.8 2.5 1.5 1.5
[0077] In Tables 1-2 above, the antioxidant is antioxidant RD, the accelerator is accelerator NS, the silane coupling agent is Si69, and the softener is environmentally friendly aromatic oil;
[0078] The preparation method of tread rubber A comprises the following steps:
[0079] S11, mixing of the first stage A masterbatch: setting the speed of the intermeshing internal mixer to 45 rpm, adding natural rubber and styrene-butadiene rubber into the intermeshing internal mixer and mixing for 45 seconds, then adding zinc oxide, carbon black, white carbon black and silane coupling agent and mixing for 155 seconds, lifting the bolt, and then pressing the bolt for 235 seconds before discharging to obtain the first stage A masterbatch;
[0080] S12, A second stage masterbatch mixing: set the speed of the shearing type internal mixer to 55rpm, add A first stage masterbatch, stearic acid, microcrystalline wax, and softener into the shearing type internal mixer, mix for 75 seconds, lift the plug, hold for 5 seconds, then press the plug and mix for 130 seconds, then lift the plug to the top, change the rotor speed to 35rpm, press the plug and mix for 165 seconds, then discharge the glue to the open mixer, this is A second stage masterbatch;
[0081] S13, set the roller pitch of the mixing mill to 2.5mm, the rotation speed to 10m / s, the cooling roller speed to 8m / s, add the second stage masterbatch and mix for 30 seconds, form a ring for 15 seconds, and swing the mixing for 160 seconds, then add sulfur, accelerator, and antioxidant, mix and swing for 245 seconds, reverse the cooling roller and break it, and remove the rubber to obtain the final mixing, thereby obtaining tread rubber A;
[0082] The preparation method of tread rubber B comprises the following steps:
[0083] S21, mixing of the first stage B masterbatch: setting the speed of the intermeshing internal mixer to 45 rpm, adding natural rubber into the intermeshing internal mixer and mixing for 45 seconds, then adding zinc oxide, carbon black, white carbon black and silane coupling agent and mixing for 155 seconds, lifting the plug, and then pressing the plug for 235 seconds before discharging to obtain the first stage B masterbatch;
[0084] S22, B second stage masterbatch mixing: set the speed of the shearing type internal mixer to 55rpm, add B first stage masterbatch, stearic acid, microcrystalline wax and softener into the shearing type internal mixer, mix for 75 seconds, lift the plug, hold for 5 seconds, then press the plug and mix for 130 seconds, then lift the plug to the top, change the rotor speed to 35rpm, press the plug and mix for 165 seconds, then discharge the rubber to the open mixer, this is B second stage masterbatch;
[0085] S23, set the roller distance of the mixing mill to 2.5mm, the rotation speed to 10m / s, the cooling roller speed to 8m / s, add the second stage masterbatch and mix for 30 seconds, make a ring for 15 seconds, and swing the mixing for 160 seconds. Then, add sulfur, accelerator and antioxidant. After mixing and swinging for 245 seconds, reverse the cooling roller and break it. The final mixing is obtained by rubber discharge to obtain tread rubber B.
[0086] The main properties of the common formulation A and other formulations of the tread rubber A in Table 1 are shown in Table 3.
[0087] Table 3 - Comparison of physical properties of tread rubber A
[0088]
[0089]
[0090] The main properties of the ordinary formulation B and other formulations of the tread rubber B in Table 2 are shown in Table 4.
[0091] Table 4 - Comparison of physical properties of tread rubber A
[0092]
[0093] In Tables 3 to 4, compression heat generation was tested according to the national standard GB / T 1687.3-2016;
[0094] The test method for cutting depth is: use a 500g blade, let it fall freely from a height of 80cm, cut the test tread rubber below to form an incision, and cut 5 times to take the average value.
[0095] Example 2
[0096] This embodiment provides an all-steel radial tire with a bionic structure tread, comprising a plurality of tread rubbers A and B that are staggered and stacked with each other;
[0097] The number of times the tread rubber A and the tread rubber B are staggered is 1, the thickness ratio of the tread rubber A to the tread rubber B is 1:1, the tread rubber A adopts the formula in Table 1, and the tread rubber B adopts the formula in Table 2.
[0098] The all-steel radial tire composed of tread rubber A and tread rubber B with different formulations in Example 2 was tested on a machine tool. The results are as follows: Figure 3 shown.
[0099] Specifically, Figure 3 The relationship between the 14.00R25 national standard 47h durability temperature measurement (according to GB / T 30193-2013) and the tread cutting depth result and the tread rubber A / B hardness difference.
[0100] from Figure 3 It can be seen that under the conditions of A / B compounding times of 1 (i.e., the number of staggered superpositions of tread rubber A and tread rubber B is 1) and thickness ratio of 1:1, the test results of temperature measurement and cutting on 14.00R25 all-steel radial tire after 47 hours of national standard durability show that when the hardness difference between tread rubber A and tread rubber B is between 2-10 and the hardness of B is between 50-70, the heat generation is relatively low when the cutting difference is not large, especially for the combination of formula 1 + formula 5, the tread temperature is 127℃, which is the lowest. At this time, the hardness difference between tread rubber A and tread rubber B is 8 degrees.
[0101] Example 3
[0102] This embodiment provides an all-steel radial tire with a bionic structure tread, comprising a plurality of tread rubbers A and B that are staggered and stacked with each other;
[0103] The number of times the tread rubber A and the tread rubber B are staggered is 1 to 5, the thickness ratio of the tread rubber A to the tread rubber B is 1:1, the tread rubber A adopts the formula 1 in Table 1, and the tread rubber B adopts the formula 5 in Table 2.
[0104] According to Example 3, the tread rubber A adopts recipe 1, the tread rubber B adopts recipe 5, the number of staggered stacking of the tread rubber A and the tread rubber B is 1 to 5, and the thickness ratio of the tread rubber A to the tread rubber B is 1:1, the effect of the number of staggered stacking on the tire temperature and cutting depth is as follows: Figure 4 shown.
[0105] Specific Figure 4 This is the relationship between the 47h temperature measurement and tread cutting depth results of the 14.00R25 national standard durability and the number of times n of the tread rubber A / B interlaced stacking.
[0106] from Figure 4 It can be seen that the tread rubbers A and B adopt the combination of formula 1 in Table 1 + formula 5 in Table 2. Under the condition that the A / B composite thickness ratio is 1:1, after 47 hours of national standard durability test, when n≥2, with the increase of the number of composite times (i.e. the number of times the tread rubbers A / B are staggered and superimposed), the tire tread temperature gradually decreases and the cutting depth decreases at the same time.
[0107] Example 4
[0108] This embodiment provides an all-steel radial tire with a bionic structure tread, comprising a plurality of tread rubbers A and B that are staggered and stacked with each other;
[0109] Among them, the number of times the tread rubber A and the tread rubber B are staggered and superimposed is 3, and the thickness ratios of the tread rubber A and the tread rubber B are 1:1, 1:2, 1:3, 1:4, 1:5, 1:0.5 (i.e. 2), 1:0.3333 (i.e. 3), 1:0.25 (i.e. 4), and 1:0.2 (i.e. 5), respectively. The tread rubber A adopts the formula 1 in Table 1, and the tread rubber B adopts the formula 5 in Table 2.
[0110] According to Example 4, the tread rubber A adopts recipe 1, the tread rubber B adopts recipe 5, the number of staggered stacking of the tread rubber A and the tread rubber B is 3, and the thickness ratio of the tread rubber A to the tread rubber B is 5 to 1 / 5, the effect of the thickness ratio of the tread rubber A to the tread rubber B on the tire temperature and the cutting depth is as follows: Figure 5 shown.
[0111] Specific Figure 5 This is the relationship between the 14.00R25 national standard 47h durability temperature measurement and tread cutting depth results and the ratio of the tread rubber A / B composite thickness.
[0112] from Figure 5 It can be seen that tread rubbers A and B adopt a combination of formula 1 in Table 1 + formula 5 in Table 2. Under the condition that the number of staggered superposition of tread rubbers A and B is 3, after 47 hours of national standard durability test, when the ratio of A / B composite thickness is 5, it has the lowest cutting depth, only 13.1mm, but the tire temperature is also the highest, reaching 164°C, and the risk of early thermal peeling is very high.
[0113] When the A / B composite thickness ratio is 1:2 and 1:5, the temperature of the tire tread is 94°C and 89°C respectively, which are both relatively low. However, when the A / B composite thickness ratio is 1:2, it has a shallower cutting depth of only 17.9mm. At this time, it has good cutting resistance and a very low tire tread temperature, greatly reducing the risk of early thermal peeling.
[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An all-steel radial tire with a bionic structural tread, It is characterized in that It includes a plurality of tread rubbers A and B which are staggered and stacked with each other; The Shore hardness of the tread rubber A is 2 to 10 degrees higher than that of the tread rubber B.
2. The all-steel radial tire with a bionic structural tread as claimed in claim 1, It is characterized in that The Shore hardness of the tread rubber B is 50 to 70 degrees.
3. The all-steel radial tire with a bionic structural tread as claimed in claim 1, It is characterized in that The number of times the tread rubber A and the tread rubber B are staggered and superimposed is ≥2.
4. The all-steel radial tire with a bionic structural tread as claimed in claim 1, It is characterized in that The thickness ratio of the tread rubber A to the tread rubber B is 1:
2.
5. The all-steel radial tire with a bionic structural tread as claimed in claim 1, It is characterized in that The Shore hardness of the tread rubber A is 8 degrees higher than that of the tread rubber B. The Shore hardness of the tread rubber B is 61 degrees. The number of times the tread rubber A and the tread rubber B are staggered and superimposed is 3.
6. The all-steel radial tire with a bionic structural tread as claimed in claim 5, It is characterized in that The materials used in the tread rubber A include the following components in parts by weight: 10-90 parts of natural rubber, 90-10 parts of styrene-butadiene rubber, 50-90 parts of carbon black, 0-15 parts of white carbon black, 2.5-6 parts of zinc oxide, 1.0-4.5 parts of stearic acid, 1-5 parts of microcrystalline wax, 1.5-5.5 parts of antioxidant, 2-8 parts of softener, 0-3 parts of silane coupling agent, 2.5-5 parts of sulfur, and 1-3.5 parts of accelerator.
7. The all-steel radial tire with a bionic structural tread as claimed in claim 5, It is characterized in that The materials used in the tread rubber B include the following components by weight: 100 parts of natural rubber, 10-30 parts of carbon black, 10-25 parts of white carbon black, 3-5 parts of zinc oxide, 2-4 parts of stearic acid, 0.5-2 parts of microcrystalline wax, 1-4 parts of antioxidant, 2-5 parts of silane coupling agent, 1-4 parts of softener, 1.5-5 parts of sulfur, and 1-3 parts of accelerator.
8. The all-steel radial tire with a bionic structural tread as claimed in claim 5, It is characterized in that The materials used in the tread rubber A include the following components in parts by weight: 80 parts of natural rubber, 20 parts of styrene-butadiene rubber, 65 parts of carbon black, 5 parts of white carbon black, 6 parts of zinc oxide, 3 parts of stearic acid, 2 parts of microcrystalline wax, 4 parts of antioxidant, 6 parts of softener, 1 part of silane coupling agent, 3 parts of sulfur, and 2 parts of accelerator. The materials used in the tread rubber B include the following components in parts by weight: 100 parts of natural rubber, 25 parts of carbon black, 15 parts of white carbon black, 5 parts of zinc oxide, 2 parts of stearic acid, 1 part of microcrystalline wax, 3 parts of antioxidant, 3 parts of silane coupling agent, 2 parts of softener, 2.5 parts of sulfur, and 1.5 parts of accelerator.
9. The all-steel radial tire with a bionic structural tread as claimed in claim 6, It is characterized in that The preparation method of the tread rubber A comprises the following steps: Add natural rubber and styrene-butadiene rubber into a meshing internal mixer, mix, add zinc oxide, carbon black, white carbon black, and silane coupling agent, continue mixing, lift the bolt, and then press the bolt and discharge the material to obtain a masterbatch of stage A; Adding the first stage A masterbatch, stearic acid, microcrystalline wax and softener into a shearing type internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and discharging the glue to obtain the second stage A masterbatch; Add the second-stage masterbatch A into the open mixing mill for mixing, and continue to add sulfur, accelerator and antioxidant, mix and discharge the rubber to obtain tread rubber A.
10. The all-steel radial tire with a bionic structural tread as claimed in claim 7, It is characterized in that The preparation method of the tread rubber B comprises the following steps: After adding natural rubber to a meshing internal mixer and mixing, zinc oxide, carbon black, white carbon black and silane coupling agent are added and mixed, the plug is lifted, and then the plug is pressed and the material is discharged to obtain a masterbatch of stage B; Adding the first stage B masterbatch, stearic acid, microcrystalline wax and softener into a shearing type internal mixer, mixing, lifting the plug, and then pressing the plug, mixing, and discharging the glue to obtain the second stage B masterbatch; Add the second-stage masterbatch B into the open mixing mill for mixing, continue to add sulfur, accelerator and antioxidant, mix and discharge the rubber to obtain tread rubber B.