Method for recovering nano-hydroxyapatite from sludge

By hydrothermal synthesis and incineration of the sludge, the target alkali liquid is used to leaching phosphorus and adding calcium source, the problem of long process flow in the existing technology is solved, and efficient and low-cost preparation of hydroxyapatite is achieved. , improves the purity and uniformity of the product.

CN119079952APending Publication Date: 2024-12-06HUAZHONG UNIV OF SCI & TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411205068.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The process of recovering phosphorus from sludge and preparing hydroxyapatite in the prior art is relatively long, and a method is needed to shorten this process.

Method used

By hydrothermal synthesis and moisture removal of the sludge added with the target additive, an absolute dry water-heat sludge was obtained, and then incinerated. The target alkali liquid was used to leache the sludge incineration ash, and then it was separated by solid-liquid and into the phosphorus-containing leaching liquid. Add calcium source to obtain hydroxyapatite.

Benefits of technology

This method effectively shortens the process flow of preparing hydroxyapatite, improves product uniformity and purity, reduces process costs, and avoids the problem of co-soluble impurity elements and heavy metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079952A_ABST
    Figure CN119079952A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sludge resource utilization, in particular to a method for recycling nano-hydroxyapatite from sludge. According to the technical scheme provided by the invention, the method comprises the following steps: sequentially carrying out hydrothermal synthesis and moisture removal on sludge added with a target additive to obtain absolutely-dry hydrothermal sludge, incinerating the absolutely-dry hydrothermal sludge to obtain sludge incineration ash, leaching the sludge incineration ash by using target alkali liquor, and carrying out solid-liquid separation to obtain a phosphorus-containing leachate, and finally, adding a calcium source into the phosphorus-containing leachate to obtain hydroxyapatite. Therefore, according to the technical scheme, the target alkali liquor is used for leaching the sludge added with the target additive to obtain phosphorus, so that the technological process for preparing the hydroxyapatite can be shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sludge resource utilization, and in particular to a method for recovering nano hydroxyapatite from sludge. Background Art

[0002] Pollutants and nutrients in sewage are aggregated by the proliferation of bacteria and chemical agents, eventually forming sludge. With the continuous development of medicine and materials science, the demand for functional materials such as artificial bones, artificial teeth, surgical implants, drug carriers and liquid chromatography separation columns is also increasing. At the same time, the output of hydroxyapatite is also rising, resulting in an increase in the demand for its production raw materials (such as phosphorus).

[0003] In the related art, the method for recovering phosphorus from sludge and preparing hydroxyapatite mainly adopts acid leaching recovery, but the process flow of this method is relatively long.

[0004] Therefore, there is an urgent need for a method for recovering nano-hydroxyapatite from sludge to solve this technical problem. Summary of the invention

[0005] The invention provides a method for recovering nano hydroxyapatite from sludge, which can shorten the process flow of preparing hydroxyapatite.

[0006] The present invention provides a method for recovering nano-hydroxyapatite from sludge, comprising:

[0007] The sludge to which the target additive is added is subjected to hydrothermal synthesis and water removal in sequence to obtain absolutely dry hydrothermal sludge;

[0008] Incinerating the absolutely dry hydrothermal sludge to obtain sludge incineration ash;

[0009] The sludge incineration ash is leached with the target alkali solution, and a phosphorus-containing leaching solution is obtained after solid-liquid separation;

[0010] A calcium source is added to the phosphorus-containing leaching solution to obtain hydroxyapatite.

[0011] As can be seen from the above scheme, the present invention provides a method for recovering nano-hydroxyapatite from sludge, by sequentially performing hydrothermal synthesis and water removal on the sludge with the target additive added, obtaining absolutely dry hydrothermal sludge, then incinerating the absolutely dry hydrothermal sludge to obtain sludge incineration ash, leaching the sludge incineration ash with the target alkali solution, and obtaining a phosphorus-containing leaching solution after solid-liquid separation, and finally adding a calcium source to the phosphorus-containing leaching solution to obtain hydroxyapatite. Therefore, the above technical scheme is to use the target alkali solution to leach the sludge with the target additive added to obtain phosphorus, so the process flow of preparing hydroxyapatite can be shortened. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0013] Figure 1 A schematic diagram of a method for recovering nano-hydroxyapatite from sludge provided in an embodiment of the present invention;

[0014] Figure 2 A comparison chart of hydroxyapatite recovered by the method provided in the embodiment of the present invention and commercial grade hydroxyapatite;

[0015] Figure 3 A thermodynamic equilibrium calculation system diagram for the precipitation reaction between impurity components in a phosphorus-containing leachate and a target phosphorus-containing product provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0017] See also Figure 1 One embodiment of the present invention provides a method for preparing hydroxyapatite based on sludge, the method comprising:

[0018] Step 100, sequentially performing hydrothermal synthesis and water removal on the sludge to which the target additive is added to obtain absolutely dry hydrothermal sludge;

[0019] Step 102, incinerating the absolutely dry hydrothermal sludge to obtain sludge incineration ash;

[0020] Step 104: leaching the sludge incineration ash with the target alkali solution, and obtaining a phosphorus-containing leaching solution after solid-liquid separation;

[0021] Step 106: adding a calcium source to the phosphorus-containing leaching solution to obtain hydroxyapatite.

[0022] In this embodiment, the sludge with the target additive added is subjected to hydrothermal synthesis and water removal in sequence to obtain absolutely dry hydrothermal sludge, and then the absolutely dry hydrothermal sludge is incinerated to obtain sludge incineration ash, and the sludge incineration ash is leached with the target alkali solution, and a phosphorus-containing leaching solution is obtained after solid-liquid separation, and finally a calcium source is added to the phosphorus-containing leaching solution to obtain hydroxyapatite. Therefore, the above technical solution is to use the target alkali solution to leach the sludge with the target additive added to obtain phosphorus, so that the process flow of preparing hydroxyapatite can be shortened.

[0023] In one embodiment of the present invention, the target additive includes at least one of a target acid solution and organic solid waste.

[0024] In one embodiment of the present invention, the target acid solution includes at least one of sulfuric acid, hydrochloric acid, nitric acid, formic acid, acetic acid, oxalic acid, citric acid and ascorbic acid.

[0025] In one embodiment of the present invention, the organic solid waste includes at least one of a first organic solid waste and a second organic solid waste, the first organic solid waste includes at least one of waste plastics containing sulfur or chlorine, medical waste and waste tires, and the second organic solid waste includes at least one of waste paper containing active ingredients, cotton and linen cloth and medicinal residues.

[0026] In this embodiment, the target additives and sludge are hydrothermally treated to regulate the form of phosphorus, promote the directional conversion of Ca / Mg-bound phosphorus and organic phosphorus to Fe / Al-bound phosphorus, and thus realize the recovery of phosphorus in the sludge.

[0027] Since the Fe / Al bound phosphorus in the sludge is soluble in alkali, but the Ca / Mg bound phosphorus is difficult to dissolve in alkali, it is necessary to convert the Ca / Mg bound phosphorus and organic phosphorus in the sludge into Fe / Al bound phosphorus by adding target additives. Studies have shown that in the slightly acidic hydrothermal process, the organic phosphorus and Ca / Mg bound phosphorus in the sludge will decompose and transform into Fe / Al bound phosphorus. Therefore, adding target additives to adjust the pH value of the sludge before hydrothermal synthesis so that the sludge has the pH environment required for the above-mentioned conversion reaction can promote the conversion of phosphorus forms to Fe / Al bound phosphorus.

[0028] Among them, the first organic solid waste containing sulfur and chlorine elements will generate acidic substances such as HCl and H2SO4 during the hydrothermal process, and the second organic solid waste containing active ingredients will generate acidic substances such as phenols, lactic acid and glycolic acid during the hydrothermal process, which can also reduce the pH of the sludge, thereby promoting the conversion of phosphorus forms into Fe / Al bound phosphorus, and at the same time realizing the resource treatment of solid waste.

[0029] In this embodiment, because the filtrate after the solid-liquid separation of the hydrothermal sludge contains unconsumed organic acid or inorganic acid, or various organic acidic substances generated by organic solid waste in the hydrothermal process. When the filtrate is used for the solid-liquid ratio adjustment in the subsequent hydrothermal process, the acidic substances therein can once again promote the directional conversion of organic phosphorus and Ca / Mg-bound phosphorus in the new sludge to Fe / Al-P. In this way, the required amount of target acid or organic solid waste can be reduced, while reducing the process cost.

[0030] In some embodiments, the sludge is mixed with the target additive and the solid-liquid ratio is adjusted to be 1:8 to 1:15. Water is used to adjust the solid-liquid ratio during the first hydrothermal synthesis, and the filtrate obtained after solid-liquid separation of the previous hydrothermal reaction is used to adjust the solid-liquid ratio during the subsequent hydrothermal process.

[0031] In some embodiments, the hydrothermal reaction temperature is 150-300° C., and the hydrothermal reaction time is 5-300 min.

[0032] In some embodiments, the incineration temperature is 750-900° C. to ensure the incineration effect of absolutely dry hydrothermal sludge.

[0033] In one embodiment of the present invention, the pH value of the product obtained by hydrothermal synthesis is 3-6.

[0034] In this embodiment, the pH value of the product obtained by hydrothermal synthesis is 3-6 to ensure that the Ca / Mg-bound phosphorus and organic phosphorus in the sludge are fully converted into Fe / Al-bound phosphorus.

[0035] In one embodiment of the present invention, the target alkali solution includes at least one of sodium hydroxide solution, potassium hydroxide solution and ammonia water.

[0036] In this embodiment, a high-concentration acid leaching method is widely used in the current process to leach phosphorus. Such a method will cause impurity elements and heavy metals to be dissolved in large quantities along with phosphorus. However, these impurity elements and heavy metal elements have poor solubility under alkaline conditions, or even do not dissolve. This means that if the target alkali solution is used for phosphorus leaching, the co-dissolution problem of impurity elements and heavy metals can be effectively avoided, thereby shortening the preparation step of hydroxyapatite. In order to achieve the above purpose, the type and concentration of the target alkali solution are optimized, and it is determined that the target alkali solution is used to leach the sludge incineration ash.

[0037] In the related art, some leachates usually use organic acid solutions or inorganic acid solutions to achieve the leaching of phosphorus, wherein the concentration of the organic acid solution or the inorganic acid solution is often greater than 0.5 mol / L. Under the aforementioned acidic leaching conditions, the main impurity elements such as Fe, Al and Mg in the sludge and heavy metal elements such as Cu, Pb, Zn, Cr and Mn will be dissolved in large quantities with the phosphorus element, and then precipitate together with the phosphorus element in the phosphorus element recovery process, reducing the purity and safety of hydroxyapatite. Secondly, in order to avoid the interference of the above impurities on the purity of hydroxyapatite, it is often necessary to remove impure ions by adjusting the pH pre-precipitation method, the cation exchange resin method, etc., and then adjust the pH to the most suitable precipitation range of hydroxyapatite to obtain the largest possible yield. This method often requires 6-8 subdivision steps to achieve purification and pH adjustment, which greatly increases the complexity and reagent cost of the entire phosphorus element recovery process. However, the target alkaline solution in this embodiment realizes the leaching of phosphorus in the sludge incineration ash, while effectively avoiding the problem of co-dissolution of impurity elements and heavy metals. This method effectively simplifies the treatment process and reduces the treatment cost.

[0038] In one embodiment of the present invention, the concentration of the target alkali solution is 0.06-0.20 mol / L, which can ensure the leaching effect of the target alkali solution on phosphorus in the sludge incineration ash.

[0039] In this embodiment, thermodynamic calculations show that under normal temperature and pressure conditions, hydroxyapatite has an independent precipitation interval under alkaline conditions above pH 11.0. Figure 3 As shown, other phosphorus-containing products (such as Fe3(PO4)2, MgNH4PO4, Ca5(PO4)3OH) and solid impurities (such as Fe(OH)3, Al(OH)3, Mg(OH)2, Ca(OH)2) cannot undergo precipitation reaction in this range. Therefore, it is only necessary to control the alkali concentration and ensure that the pH of the leaching solution is within this range to theoretically achieve the separate precipitation of Ca5(PO4)3OH, thereby ensuring its purity.

[0040] In some embodiments, the solid-liquid ratio of the sludge incineration ash to the target alkali solution is 1:50 to 1:200, the leaching time is 2 to 4 hours, and the tumbling oscillation rate is 60 to 200 rpm.

[0041] In one embodiment of the present invention, the phosphorus-containing leaching solution is used for circulating leaching of the incineration ash of new absolute dry hydrothermal sludge. When the pH value of the phosphorus-containing leaching solution is less than 11, the circulating leaching of the phosphorus-containing leaching solution is stopped.

[0042] In this embodiment, the phosphorus-containing leaching solution is recycled to the new absolutely dry hydrothermal sludge incineration ash for cyclic leaching of phosphorus, which can reduce reagent consumption.

[0043] In some embodiments, the phosphorus-containing leachate may be filtered using a 0.45 μm filter head to remove solid particles that have not been separated.

[0044] In one embodiment of the present invention, after obtaining the phosphorus-containing leachate after solid-liquid separation and before adding the calcium source to the phosphorus-containing leachate, the process further comprises:

[0045] An impurity remover is added to the phosphorus-containing leaching solution to remove arsenic and copper elements in the phosphorus-containing leaching solution by using the impurity remover to obtain a purified phosphorus-containing leaching solution.

[0046] In this embodiment, the impurity remover is used to remove the arsenic and copper elements in the phosphorus-containing leaching solution to ensure the purity of the hydroxyapatite.

[0047] In one embodiment of the present invention, the impurity remover is ammonium sulfide, and the molar amount of sulfur in the ammonium sulfide is 1.5 times the sum of the molar amount of arsenic and the molar amount of copper in the phosphorus-containing leachate.

[0048] In one embodiment of the present invention, step 106 may specifically include:

[0049] adding a calcium source to the purified phosphorus-containing leachate and stirring the mixture to obtain a mixed solution;

[0050] Allow the mixed solution to stand for curing;

[0051] Performing solid-liquid separation on the mixed solution after static curing to obtain a solid product;

[0052] Washing the solid product with deionized water, and freeze-drying the washed solid product;

[0053] The freeze-dried solid product was calcined under air atmosphere to obtain hydroxyapatite.

[0054] In this embodiment, the obtained hydroxyapatite is in the form of fine particles at the microscopic level, with particle sizes ranging from tens of nanometers to hundreds of nanometers, and the Ca, P, and O elements are uniformly distributed. Figure 2 As shown, in Figure 2 In the figure, a and b are respectively the macroscopic morphology comparisons of the hydroxyapatite obtained by the method and the commercial grade hydroxyapatite, c and d are respectively the microscopic morphology comparisons of the hydroxyapatite obtained by the method and the commercial grade hydroxyapatite, e is the element distribution uniformity test of the hydroxyapatite obtained by the method, and f is the crystal structure comparison of the hydroxyapatite recovered by the method and the commercial grade hydroxyapatite. Figure 2 It can be seen that the hydroxyapatite prepared in the embodiment of the present invention has greatly improved uniformity.

[0055] In addition, the impurity content of hydroxyapatite can reach the liquid chromatography column standard (Biorad CHT Part 2.4: Purity), the raw material standard of surgical implants (GB / T23101.6) and the commercial grade reagent standard. The data are shown in Table 1 (showing high-resolution liquid chromatography column grade, surgical implant raw materials, commercial grade, analytical grade reagents and the recovered product of this method).

[0056] Table 1 Comparison of hydroxyapatite and standard limits

[0057]

[0058]

[0059] In some embodiments, the mixed solution is stirred at a speed of 60 to 200 rpm for a time of 10 to 60 min, and then the stirring is stopped.

[0060] In some embodiments, the mixed solution may be allowed to stand for 0.5 to 24 hours.

[0061] In some embodiments, vacuum filtration is used to separate the solid from the liquid in the mixed solution, so that the mixed solution can be better separated from the solid and the liquid.

[0062] In some embodiments, the solid product is washed three times with deionized water to remove impurity ions in the solid product.

[0063] In some embodiments, the burning temperature may be 700-900° C., and the burning time may be 0.5-2 h to ensure that the solid product after freeze-drying is fully burned.

[0064] In one embodiment of the present invention, the calcium source includes at least one of solid powdered CaCl2 and Ca(NO3)2, and the molar ratio of the calcium source to the phosphorus element in the phosphorus-containing leachate is 1.667:1.

[0065] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering nano-hydroxyapatite from sludge, characterized in that: include: The sludge to which the target additive is added is subjected to hydrothermal synthesis and water removal in sequence to obtain absolutely dry hydrothermal sludge; Incinerating the absolutely dry hydrothermal sludge to obtain sludge incineration ash; The sludge incineration ash is leached with the target alkali solution, and a phosphorus-containing leaching solution is obtained after solid-liquid separation; A calcium source is added to the phosphorus-containing leaching solution to obtain hydroxyapatite.

2. The method according to claim 1, characterized in that The target additive includes at least one of a target acid solution and organic solid waste, and the target acid solution includes at least one of sulfuric acid, hydrochloric acid, nitric acid, formic acid, acetic acid, oxalic acid, citric acid and ascorbic acid.

3. The method according to claim 2, characterized in that The organic solid waste includes at least one of a first organic solid waste and a second organic solid waste, wherein the first organic solid waste includes at least one of waste plastics containing sulfur or chlorine, medical waste and waste tires, and the second organic solid waste includes at least one of waste paper containing active ingredients, cotton and linen cloth and medicinal residues.

4. The method according to claim 3, characterized in that The pH value of the product obtained by hydrothermal synthesis is 3-6.

5. The method according to claim 1, characterized in that The target alkali solution includes at least one of a sodium hydroxide solution, a potassium hydroxide solution and an ammonia solution, and the concentration of the target alkali solution is 0.06 to 0.20 mol / L.

6. The method according to claim 1, characterized in that The phosphorus-containing leaching solution is used for circulating leaching of the incineration ash of new absolute dry hydrothermal sludge. When the pH value of the phosphorus-containing leaching solution is less than 11, the circulating leaching of the phosphorus-containing leaching solution is stopped.

7. The method according to claim 1, characterized in that After obtaining the phosphorus-containing leachate after solid-liquid separation and before adding the calcium source to the phosphorus-containing leachate, the method further comprises: An impurity remover is added to the phosphorus-containing leachate to remove arsenic and copper elements in the phosphorus-containing leachate by using the impurity remover to obtain a purified phosphorus-containing leachate.

8. The method according to claim 7, characterized in that The impurity remover is ammonium sulfide, and the molar amount of sulfur in the ammonium sulfide is the sum of 1.5 times the molar amount of arsenic element and the molar amount of copper element in the phosphorus-containing leachate.

9. The method according to any one of claims 1 to 8, characterized in that The step of adding a calcium source to the phosphorus-containing leachate to obtain hydroxyapatite comprises: adding a calcium source to the purified phosphorus-containing leachate and stirring the mixture to obtain a mixed solution; Allowing the mixed solution to stand for curing; Performing solid-liquid separation on the mixed solution after static curing to obtain a solid product; Washing the solid product with deionized water, and freeze-drying the washed solid product; The freeze-dried solid product was calcined under air atmosphere to obtain hydroxyapatite.

10. The method according to claim 9, characterized in that The calcium source includes at least one of solid powdered CaCl2 and Ca(NO3)2, and the molar ratio of the calcium source to the phosphorus element in the phosphorus-containing leachate is 1.667:1.

Citation Information

Patent Citations

  • Preparation method for phosphorus-containing sludge-based carbon material with high bioavailability

    CN107857245A

  • Method for extracting phosphorus element from sewage sludge

    CN112678790A

  • Method for efficiently recovering phosphorus from municipal sludge and synchronously preparing porous biochar

    CN113072267A

  • Method and system for sludge modification and phosphorus fixation and method and system for recycling phosphorus based on incineration ash acid leaching

    CN115159489A

  • Method for preparing pyrolytic carbon with high biological available phosphorus content from calcium-based conditioning excess sludge

    CN116514095A