Iron-containing ZSM-5 molecular sieve as well as preparation method and application thereof
The use of peroxide for synthesizing iron-containing ZSM-5 molecular sieves addresses the challenges of metal encapsulation in silicon-aluminum MFI molecular sieves, achieving clean production and improved catalytic performance by evenly distributing iron within the molecular sieve framework, thereby enhancing light olefin selectivity.
Patent Information
- Application Number
- CN202310637619.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Existing methods for encapsulating metals into silicon-aluminum MFI molecular sieves face challenges such as hydroxide precipitation and interaction with phosphorus, leading to synthesis difficulties and low activity, while the use of amine nitrogen ligands results in organic wastewater discharge.
A method using peroxide to synthesize iron-containing ZSM-5 molecular sieves, encapsulating metals without amine nitrogen organic matter, thereby avoiding wastewater discharge and achieving clean production.
The method enables the encapsulation of iron into ZSM-5 molecular sieves, improving catalytic performance by distributing iron active components evenly within the molecular sieve framework, enhancing catalytic cracking reactions and increasing the conversion rate and selectivity of light olefins.
Smart Images

Figure CN119080019A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to an iron-containing ZSM-5 molecular sieve and a preparation method and application thereof. Background Art
[0002] Catalytic cracking refers to the process of converting hydrocarbons into low-carbon olefins such as ethylene, propylene and butene under the action of a catalyst, and producing light aromatics at the same time. The process of producing low-carbon olefins by catalytic cracking of heavy oil has always occupied a large share of the low-carbon olefin market due to its strong raw material adaptability and low production cost. Since the mid-1980s, Sinopec Research Institute of Petroleum and Chemical Industry (Sinopec Research Institute) has been tracking and studying this technology. In 1994, the Research Institute of Petroleum and Chemical Industry developed a catalytic cracking (DCC) process for producing low-carbon olefins using heavy oil (vacuum distillate oil, coking gas oil and residual oil, etc.) as raw materials. After the successful industrialization of DCC technology, the Research Institute of Petroleum and Chemical Industry developed a catalytic thermal cracking (CPP) process for directly producing ethylene and propylene from heavy oil, which has multiple production schemes such as maximum ethylene, maximum propylene and simultaneous production of ethylene and propylene. Compared with the steam cracking process, the CPP process broadens the source of ethylene raw materials and reduces the cost of ethylene raw materials. At the same time, the reaction temperature is lower than that of the steam cracking process, so the energy consumption of the device is significantly reduced. Light oil catalytic cracking mainly refers to the process of producing ethylene and propylene from light gasoline or naphtha in the presence of a catalyst. This process can realize the transformation of petroleum resources into basic chemical raw materials and will play an important role in future chemical refineries.
[0003] The development of catalysts is considered to be one of the core contents of the research and development of catalytic cracking technology. Early research on catalytic cracking catalysts focused on metal oxides. The catalysts used in the catalytic cracking technology that has been industrially applied are basically based on zeolite molecular sieves as active components. ZSM-5 molecular sieve is a silicon-aluminum type MFI molecular sieve. Due to its unique three-dimensional ten-membered ring channel structure and suitable acid properties, it shows good propylene selectivity. At the same time, due to its good hydrothermal stability and good inhibition of coke precursors, it is considered to be one of the most promising active components of catalytic cracking catalysts. The acid properties of molecular sieves include acid type, acid amount, acid strength and acid center distribution. Element modification is a simple and effective method to adjust the acidity of molecular sieves. Studies have modified ZSM-5 molecular sieves with alkaline earth metals such as Mg, Ca, Ba and Sr. It was found that the introduction of alkaline earth metals promoted the transformation of some strong acid sites into weak acid sites. When n-butane was used as a reactant, the introduction of Ba obtained the highest ethylene and propylene yields, while the aromatic yield decreased significantly, which may be due to the inhibition of hydrogen transfer reactions.
[0004] Encapsulation is an important way to introduce metal components into molecular sieves. Encapsulation can not only make the metal components evenly dispersed in the molecular sieve, but also use the shape selectivity of the molecular sieve to activate the terminal carbon-hydrogen bonds of alkanes and selectively dehydrogenate, thereby reducing the methane content and increasing the selectivity of light olefins. Studies have reported the direct synthesis of MFI molecular sieves encapsulating metal Pd using ethylenediamine as a ligand, realizing the direct synthesis of high-silicon molecular sieves encapsulating metals. However, there have been many studies on encapsulating metals into all-silicon or high-silicon MFI molecular sieves, but there have been fewer studies on encapsulating metals into silicon-aluminum MFI molecular sieves. This is because if the metal is directly introduced into the synthesis system, the metal is easy to form hydroxide precipitation in an alkaline environment. In addition, the metal easily interacts with phosphorus, resulting in difficulty in synthesis or low activity. The ligand-assisted method is one of the methods for synthesizing encapsulated metal silicon-aluminum MFI molecular sieves. The criterion for selecting ligands is that the complex ion product constant is less than the metal oxide solubility product constant to achieve the complex state of the metal. Therefore, an alcohol amine complex that can be complexed with iron nitrate is selected as a ligand to form a metal complex, thereby protecting the metal and not affecting the synthesis system of the molecular sieve. However, the ligand-assisted method generally uses organic reagents as ligands, such as alcohol amine complexes, hexamethylenediamine, etc., and there are still problems such as organic wastewater discharge.
[0005] In 2016, Professor Yu Jihong's research group at Jilin University discovered the existence of hydroxyl radicals in the hydrothermal synthesis system of molecular sieves. They also found that introducing hydroxyl radicals into the synthesis system of molecular sieves can significantly accelerate the crystallization process of molecular sieves. Summary of the invention
[0006] The purpose of the present disclosure is to provide an iron-containing ZSM-5 molecular sieve and a preparation method and application thereof. The method of the present disclosure uses peroxide to synthesize encapsulated molecular sieves, encapsulates metals into ZSM-5 molecular sieves, does not use amine nitrogen organic matter and amine nitrogen ligands, avoids the discharge of amine nitrogen wastewater, and thus realizes the clean production of encapsulated iron ZSM-5 molecular sieves throughout the process.
[0007] In order to achieve the above object, the present disclosure provides a method for preparing an iron-containing ZSM-5 molecular sieve in a first aspect, the method comprising:
[0008] S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal and water to obtain a first mixture;
[0009] S2, mixing the iron source, peroxide, water and the first mixture and performing a hydrothermal reaction;
[0010] Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent.
[0011] Optionally, step S2 includes:
[0012] SS1. Mixing the iron source, peroxide and water to obtain a second mixture; the molar ratio of the iron source, peroxide and water in terms of Fe2O3 is 1:(0.2-2.5):(200-1400); preferably 1:(0.3-2.0):(200-800);
[0013] SS2. The first mixture and the second mixture are mixed and then subjected to the hydrothermal reaction; the molar ratio of the first mixture calculated as Al2O3 to the second mixture calculated as Fe2O3 is 1:(0.01-3.0); preferably 1:(0.4-2.3).
[0014] Optionally, in step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is (20-300):1:(2-30):(300-2500), preferably (35-60):1:(4-20):(500-1000);
[0015] Calculated as SiO2, the amount of the seed crystal used is 5-15 wt%, preferably 7-12 wt%, relative to the total weight of the silicon source.
[0016] Optionally, in step S2, the conditions of the hydrothermal reaction include: temperature of 150-220° C., and time of 8-32 h.
[0017] Optionally, the method further comprises: subjecting the product obtained by the hydrothermal treatment to ammonium exchange and calcination treatment; the calcination treatment conditions comprise: a temperature of 400-800° C., a time of 0.5-8 h, and an atmosphere of air or water vapor.
[0018] Optionally, in step S1, the silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate;
[0019] The aluminum source includes one or more of sodium metaaluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate;
[0020] The alkali source includes sodium hydroxide and / or potassium hydroxide;
[0021] The seed crystals include one or more ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, and the average particle size of the ZSM-5 molecular sieve is 0.5-2 μm;
[0022] The iron source is selected from one or more of ferric nitrate, ferric oxalate, ferric sulfate and ferric hydroxide.
[0023] The second aspect of the present disclosure provides an iron-containing ZSM-5 molecular sieve prepared by the method provided in the first aspect of the present disclosure.
[0024] Optionally, the iron-containing ZSM-5 molecular sieve has a structure in which an iron active component is encapsulated inside the ZSM-5 molecular sieve; and the iron active component is distributed on the framework of the ZSM-5 molecular sieve.
[0025] Optionally, the specific surface area of the iron-containing ZSM-5 molecular sieve is 200-450m 2 / g, with a total pore volume of 0.130-0.24 cm 3 ·g -1 , the micropore volume is 0.100-0.20cm 3 ·g -1 , the mesopore volume is 0.010-0.10cm 3 ·g -1 , relative crystallinity is 80-100%;
[0026] In the iron-containing ZSM-5 molecular sieve, the molar ratio of SiO2 to Al2O3 is 20-300;
[0027] Relative to the total weight of the iron-containing ZSM-5 molecular sieve, the content of the iron active component calculated as Fe2O3 is 1-3% by weight.
[0028] The third aspect of the present disclosure provides an application of the iron-containing ZSM-5 molecular sieve provided in the first aspect of the present disclosure in a catalytic cracking reaction of n-tetradecane.
[0029] Optionally, the conditions of the catalytic cracking reaction include: a temperature of 500-680°C, a reaction mass space velocity of 20-40h-1, a reaction pressure of 0.8-1.2MPa, and a catalyst-oil weight ratio of 1-1.8. Through the above technical scheme, the method disclosed in the present invention uses peroxide to synthesize encapsulated molecular sieves, encapsulates metals into ZSM-5 molecular sieves, does not use amine nitrogen organic matter and amine nitrogen ligands, avoids the discharge of amine nitrogen wastewater, and thus realizes the clean production of encapsulated iron ZSM-5 molecular sieves throughout the process.
[0030] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0032] Figure 1 is an X-ray diffraction spectrum of the iron-containing ZSM-5 molecular sieve prepared in Example 1 of the present disclosure;
[0033] Figure 2is a transmission electron microscope photograph of the iron-containing ZSM-5 molecular sieve prepared in Example 1 of the present disclosure;
[0034] Figure 3 is a STEM-Mapping photo of the iron-containing ZSM-5 molecular sieve prepared in Example 1 of the present disclosure;
[0035] Figure 4 is an X-ray diffraction spectrum of the iron-containing ZSM-5 molecular sieve prepared in Example 2 of the present disclosure;
[0036] Figure 5 is an X-ray diffraction spectrum of the iron-containing ZSM-5 molecular sieve prepared in Example 3 of the present disclosure;
[0037] Figure 6 It is the H2-TPR graph of the iron-containing ZSM-5 molecular sieve sample C and the comparative sample D1 prepared in Example 3 and Comparative Example 1 of the present disclosure. DETAILED DESCRIPTION
[0038] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.
[0039] A first aspect of the present disclosure provides a method for preparing an iron-containing ZSM-5 molecular sieve, the method comprising: S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal and water to obtain a first mixture; S2, mixing an iron source, a peroxide, water and the first mixture and then performing a hydrothermal reaction; wherein the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent.
[0040] The method disclosed in the present invention uses peroxide to synthesize molecular sieves instead of using a template agent containing amine nitrogen, thereby avoiding the discharge of amine nitrogen wastewater, thereby achieving clean production of iron-containing ZSM-5 molecular sieves.
[0041] In a preferred embodiment of the present disclosure, the peroxide is sodium persulfate or hydrogen peroxide, more preferably sodium persulfate. The peroxide can interact with the metal and the molecular sieve precursor at the same time, promote the nucleation of the molecular sieve around the metal, and encapsulate the metal into the interior of the molecular sieve.
[0042] In a specific embodiment of the present disclosure, step S2 includes: SS1, mixing the iron source, peroxide and water to obtain a second mixture; the molar ratio of the iron source, peroxide and water in terms of Fe2O3 is 1: (0.2-2.5): (500-1400); preferably 1: (0.3-2.0): (800-1200); further preferably 1: (0.5-1.8): (800-1000); SS2, mixing the first mixture with the second mixture and then performing the hydrothermal reaction; the molar ratio of the first mixture in terms of Al2O3 to the second mixture in terms of Fe2O3 is 1: (0.01-3.0); preferably 1: (0.4-2.3). Within the above-mentioned dosage ratio, the second mixture can be free of free iron ions or ferrous ions, thereby avoiding the presence of aggregated iron active components in the prepared molecular sieve and further improving its catalytic performance.
[0043] In a specific embodiment of the present disclosure, in step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is (20-300):1:(2-30):(300-2500), preferably (35-60):1:(4-20):(500-1000); calculated as SiO2, relative to the total weight of the silicon source, the amount of the seed crystal is 5-15% by weight, preferably 7-12% by weight.
[0044] According to the present disclosure, hydrothermal treatment is well known to those skilled in the art and can be carried out in equipment well known to those skilled in the art, such as a closed heat-resistant and pressure-resistant reactor. In a specific embodiment of the present disclosure, in step S2, the conditions of the hydrothermal reaction include: a temperature of 150-220°C and a time of 8-32h; preferably, a temperature of 150-180°C and a time of 8-20h. The present disclosure does not specifically limit the pressure of the hydrothermal reaction, for example, it can be carried out under the autogenous pressure of the reaction system or under an applied pressure, preferably, under the autogenous pressure of the reaction system.
[0045] In a specific embodiment of the present disclosure, the method further includes: exchanging ammonium and calcining the solid product obtained by the hydrothermal treatment; the conditions of the calcination treatment include: a temperature of 400-800°C, a time of 0.5-8h, and an atmosphere of air atmosphere or water vapor atmosphere; preferably, the temperature is 500-600°C and the time is 2-4h. The calcination treatment is well known to those skilled in the art, and can be carried out in a muffle furnace, a tubular furnace, etc. In a preferred embodiment, the solid product is washed to neutrality before exchanging ammonium, and the liquid used for washing can be any type of liquid that does not react with the solid product, for example, it can be deionized water. In another preferred specific embodiment, the solid obtained by the ammonium exchange is dried before calcination, and the drying conditions can include: a temperature of 100-150°C and a time of 5-20h.
[0046] In a specific embodiment of the present disclosure, the solid product obtained by the hydrothermal treatment can be taken out by centrifugal separation, precipitation and the like.
[0047] According to the present disclosure, the silicon source, aluminum source and alkali source are well known to those skilled in the art. In a specific embodiment of the present disclosure, the silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate; the aluminum source includes one or more of sodium aluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate; the alkali source includes sodium hydroxide and / or potassium hydroxide.
[0048] According to the present disclosure, the iron source may be a water-soluble iron salt and / or ferrous salt. In a specific embodiment of the present disclosure, the iron source is selected from one or more of ferric nitrate, ferric oxalate, ferric sulfate and ferric hydroxide.
[0049] In a specific embodiment of the present disclosure, the seed crystal includes one or more of the ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, for example, including but not limited to ZPR molecular sieve, ZSP molecular sieve, etc.; the average particle size of the ZSM-5 molecular sieve is 0.5-2μm, preferably 1-2μm. The average particle size of the ZSM-5 molecular sieve in the present disclosure refers to the average particle size of the molecular sieve estimated by SEM analysis of the molecular sieve and measuring the particle size of 50 particles randomly selected in the SEM photo to obtain the average value, and the SEM instrument model is HITACHI S-4800.
[0050] The second aspect of the present disclosure provides an iron-containing ZSM-5 molecular sieve prepared by the method provided in the first aspect of the present disclosure.
[0051] In a specific embodiment of the present disclosure, the iron-containing ZSM-5 molecular sieve has a structure in which an iron active component is encapsulated inside the ZSM-5 molecular sieve; the iron active component is distributed on the framework of the ZSM-5 molecular sieve.
[0052] In the present disclosure, “iron active components are distributed on the framework of the ZSM-5 molecular sieve” means that at least part of the Si and Al on the framework of the ZSM-5 molecular sieve is replaced by Fe. The introduction of iron elements can adjust the acid properties of the ZSM-5 molecular sieve, improve its catalytic function of cracking and dehydrogenation, and introduce the iron active components into the interior of the molecular sieve in an encapsulated manner, further reducing the severity of the catalytic cracking reaction of light hydrocarbons, and improving the conversion rate of saturated hydrocarbons and the selectivity of light olefins. In a specific embodiment of the present disclosure, the specific surface area of the iron-containing ZSM-5 molecular sieve is 200-450m 2 / g, preferably 300-400m 2 / g, with a total pore volume of 0.130-0.24 cm 3 ·g -1 , preferably 0.18-0.22cm 3 ·g -1 , the micropore volume is 0.100-0.200cm 3 ·g -1 , preferably 0.120-0.180cm 3 ·g -1 , the mesopore volume is 0.010-0.10cm 3 ·g -1 , preferably 0.030-0.080cm 3 ·g -1 , the relative crystallinity is 80-100%, preferably 85-100%; in the iron-containing ZSM-5 molecular sieve, the molar ratio of SiO2 to Al2O3 is 20-300, preferably 27-50; relative to the total weight of the iron-containing ZSM-5 molecular sieve, the content of the iron active component in terms of Fe2O3 is 0.5-3% by weight, preferably 1-3% by weight, and more preferably 1-1.5% by weight. Wherein, the molar ratio of SiO2 to Al2O3 can be obtained by X-ray fluorescence spectroscopy. The relative crystallinity is obtained by using a Siemens D5005 X-ray diffractometer with the standard sample of the ZSM-5 molecular sieve of the Petrochemical Research Institute as the benchmark (i.e., the relative crystallinity of the standard sample of the ZSM-5 molecular sieve of the Petrochemical Research Institute of China Petrochemical Corporation is 100%). The specific surface area and pore volume parameters can be determined by using a specific surface area tester based on the N2 adsorption principle and the BET calculation method (see Petrochemical Analysis Method (RIPP Test Method), RIPP151-90, Science Press, published in 1990). The content of the active iron component in terms of Fe2O3 is obtained by X-ray fluorescence spectroscopy.
[0053] The third aspect of the present disclosure provides an application of the iron-containing ZSM-5 molecular sieve provided in the second aspect of the present disclosure in a catalytic cracking reaction of n-tetradecane. In a specific embodiment of the present disclosure, the conditions of the catalytic cracking reaction include: a temperature of 500-680°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, the agent-oil weight ratio is 1-2; preferably, the temperature is 540-600℃, the reaction mass space velocity is 20-40h -1 , the reaction pressure is 1-1.2MPa, and the agent-oil weight ratio is 1.28-1.92.
[0054] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.
[0055] Silicon-aluminum molar ratio: that is, the molar ratio of SiO2 to Al2O3, tested by X-ray fluorescence spectrometry, the instrument model is Japan Rigaku Electric Co., Ltd. 3013 X-ray fluorescence spectrometer; test conditions: tungsten target, excitation voltage 40kV, excitation current 50mA;
[0056] Relative crystallinity: measured by Siemens D5005 X-ray diffractometer, with ZSM-5 molecular sieve standard sample of Petrochemical Research Institute as the benchmark (i.e., the relative crystallinity of ZSM-5 molecular sieve standard sample of Petrochemical Research Institute of China Petrochemical Corporation is 100%);
[0057] Specific surface area: determined by using a specific surface area tester based on the N2 adsorption principle and the BET calculation method (see Petrochemical Analysis Method (RIPP Test Method), RIPP151-90, Science Press, published in 1990);
[0058] Pore volume test method: The sample was vacuumed to 1.33×10 at 350°C. -2 Pa, constant temperature and pressure for 15 hours. Tests were conducted at liquid nitrogen temperature of -196°C to measure the adsorption and desorption of N2 under different relative pressures (p / p0). The desorption branch data were calculated using the BJH (Barrett-Joyner-Halenda) method to obtain the pore size distribution data of the sample;
[0059] The transmission electron microscope instrument model is JEM-2100 (200 kV) transmission electron microscope of JEOL Ltd.; the test conditions are: the acceleration voltage is 200 kV, and after the sample is processed, the grain morphology and size of the molecular sieve sample are observed at a magnification of 5000-30000;
[0060] STEM-Mapping test method and instrument: JEOL Ltd. JEM-2100 (200kV) transmission electron microscope. The accelerating voltage of the electron microscope is 200kV. Anhydrous ethanol is dispersed in the sample, and then dripped on the sample net with a diameter of 3mm for observation and testing;
[0061] H2-TPR test method and instrument: Micromeritic AutochemⅡ2920 programmed temperature desorber. Weigh 0.2g (20-40 mesh) of hydrogen molecular sieve catalyst into a sample tube, place it in a thermal conductivity cell heating furnace, use He gas as the carrier gas (25mL / min), heat it to 550℃ at a rate of 20℃ / min, and purge for 60min to remove impurities adsorbed on the catalyst surface. Then cool it to 150℃, keep the temperature constant for 60min, switch to H2-He mixed gas (10.02% H2+89.98% He) for adsorption for 60min, and continue to purge with He gas for 120min until the baseline is stable. Program the temperature to 550℃ at a heating rate of 10℃ / min for desorption. Keep it for 30min, and the desorption is completed. Use a TCD detector to detect changes in gas composition;
[0062] Test method for the content of active iron components in terms of Fe2O3: Semi-quantitative analysis of iron is performed by measuring the intensity of characteristic spectral lines of each element through XRF.
[0063] Example 1
[0064] This example uses the following steps to prepare iron-containing ZSM-5 molecular sieve A:
[0065] (1) adding 0.99 g of sodium hydroxide, 40.8 g of deionized water, 20 g of silica gel, 6.78 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.97 g of ZSM-5 seed crystals in sequence under stirring, and stirring well to obtain a first mixture;
[0066] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide and water is 55:1:4.68:589; the amount of ZSM-5 seed crystals used is 10 weight % relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0067] (2) dissolving 1.13 g of ferric nitrate nonahydrate in 10 g of deionized water, adding 0.14 g of sodium persulfate, and stirring thoroughly until a clear and transparent state is obtained to obtain a second mixture;
[0068] The molar ratio of the iron source calculated as Fe2O3, sodium persulfate and water is 1:0.2:200, and the molar ratio of the aluminum source calculated as Al2O3 to the iron source calculated as Fe2O3 is 1:0.40;
[0069] (3) adding the second mixture to the first mixture, mixing thoroughly and then transferring to a stainless steel kettle for hydrothermal treatment at 170° C. for 12 h;
[0070] (4) The product obtained by the hydrothermal treatment in step (3) was filtered, washed to a pH of 7-8, and ammonium exchanged, dried at 120° C. for 12 h, and then calcined at 550° C. for 2 h in an air atmosphere to obtain an iron-containing ZSM-5 molecular sieve, denoted as A. The structural parameters are listed in Table 1, the X-ray diffraction spectrum is shown in 1, and the transmission electron microscope photo is shown in Figure 2 , STEM-Mapping photos see Figure 3 .
[0071] Example 2
[0072] The iron-containing ZSM-5 molecular sieve B was prepared by the same method as in Example 1, except that in step (2), 1.13 g of ferric nitrate nonahydrate was dissolved in 10 g of deionized water, 0.576 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture. The molar ratio of the iron source, sodium persulfate and water in terms of Fe2O3 was 1:0.8:200, and an encapsulated iron ZSM-5 molecular sieve was obtained, which was denoted as B. The structural parameters are listed in Table 1, and its X-ray diffraction spectrum is shown in Table 4.
[0073] Example 3
[0074] The iron-containing ZSM-5 molecular sieve C was prepared by the same method as in Example 1, except that in step (2), 1.13 g of ferric nitrate nonahydrate was dissolved in 10 g of deionized water, 1.15 g of sodium persulfate was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture. The molar ratio of the iron source, sodium persulfate and water in terms of Fe2O3 was 1:1.6:200, and an encapsulated iron ZSM-5 molecular sieve was obtained, which was denoted as C. The structural parameters are listed in Table 1, its X-ray diffraction spectrum is shown in Table 5, and its H2-TPR diagram is shown in Table 1. Figure 6 .
[0075] Example 4
[0076] The same method as in Example 1 was used to prepare the iron-containing ZSM-5 molecular sieve D, except that in step (2), 1.13 g of ferric nitrate nonahydrate was dissolved in 10 g of deionized water, 0.095 g of hydrogen peroxide was added, and the mixture was stirred until it was clear and transparent to obtain a second mixture. The molar ratio of the iron source, hydrogen peroxide and water in terms of Fe2O3 was 1:1:200, and the encapsulated iron ZSM-5 molecular sieve was obtained, which was denoted as D, and the structural parameters are listed in Table 1.
[0077] Example 5
[0078] The iron-containing ZSM-5 molecular sieve E was prepared by the same method as in Example 3, except that in step (2), 1.13 g of ferric nitrate nonahydrate was dissolved in 10 g of deionized water, 1.80 g of sodium persulfate was added, the second mixture contained free iron ions, and the molar ratio of the iron source, sodium persulfate and water in terms of Fe2O3 was 1:2.5:200. The structural parameters are listed in Table 1.
[0079] Example 6
[0080] The iron-containing ZSM-5 molecular sieve G was prepared by the same method as in Example 3, except that in step (1), 0.79 g of sodium hydroxide, 56.63 g of deionized water, 13 g of silica gel, 3.45 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.38 g of ZSM-5 seed crystals were added in sequence under stirring, and the mixture was stirred well to obtain a first mixture;
[0081] In step (2), 1.13 g of ferric nitrate nonahydrate is dissolved in 10 g of deionized water, 0.14 g of sodium persulfate is added, and the mixture is stirred until it becomes clear and transparent to obtain a second mixture;
[0082] Among them, the molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide and water is 70:1:5.95:1400; calculated as SiO2, the amount of ZSM-5 seed crystals used is 7 weight% relative to the total weight of the silicon source; the silicon-to-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2μm.
[0083] Comparative Example 1
[0084] This comparative example illustrates the difference of the parent ZSM-5 molecular sieve which does not contain iron.
[0085] (1) adding 0.99 g of sodium hydroxide, 50.8 g of deionized water, 20 g of silica gel, 6.78 g of low-alkali sodium aluminate (Na2O: 153.5 g / L, Al2O3: 102.5 g / L), and 1.97 g of ZSM-5 seed crystals in sequence under stirring, and stirring well to obtain a first mixture; after stirring well, transferring the mixture to a stainless steel kettle, and performing hydrothermal treatment at 170° C. for 12 h;
[0086] The molar ratio of silicon source calculated as SiO2, aluminum source calculated as Al2O3, alkali source calculated as alkali metal oxide and water is 55:1:4.68:589; the amount of ZSM-5 seed crystals used is 10 weight % relative to the total weight of the silicon source calculated as SiO2; the silicon-aluminum ratio of the ZSM-5 seed crystals is 27, and the average particle size is 1-2 μm;
[0087] (2) The product obtained by the hydrothermal treatment in step (1) was filtered, washed to pH = 7-8, and ammonium exchanged, dried at 120°C for 12 hours, and then calcined at 550°C for 2 hours in an air atmosphere to obtain a parent ZSM-5 molecular sieve, denoted as D1, with structural parameters listed in Table 1 and its H2-TPR diagram shown in Figure 6 .
[0088] Comparative Example 2
[0089] The iron-containing ZSM-5 molecular sieve D2 was prepared in the same manner as in Example 1, except that sodium persulfate was not added. Its structural parameters are listed in Table 1.
[0090] Comparative Example 3
[0091] This comparative example illustrates the difference in the synthesis of iron-containing ZSM-5 molecular sieves using triethanolamine by the ligand-assisted method.
[0092] The iron-containing ZSM-5 molecular sieve D3 was prepared by the same method as in Example 1, except that sodium persulfate was replaced by triethanolamine, wherein the amount of triethanolamine used was 0.42 g, and the molar ratio of the iron source, triethanolamine and water calculated as Fe2O3 was 1:1:200. The structural parameters are listed in Table 1.
[0093] Test Example 1
[0094] The iron-containing ZSM-5 molecular sieves prepared in the examples and comparative examples were subjected to aging treatment. The specific aging treatment method is as follows: the aging furnace is a hydrothermal aging device made by the Institute of Petroleum Science and Technology, and the state after aging at 800°C for 17 hours is used to simulate the balance agent in industrial operation.
[0095] The ZSM-5 molecular sieve prepared in the embodiment and the comparative example was used as a catalyst in the catalytic cracking reaction to carry out the catalytic cracking reaction of n-tetradecane. The specific method is as follows: the reaction is carried out in a fixed bed reactor, the feed oil is n-tetradecane, the carrier gas is nitrogen, the flow rate is 30 mL / min, the reaction temperature is 550°C, the regeneration temperature is 600°C, the reaction pressure is 0.1 MPa, and the weight space velocity is 20 hr -1 The molecular sieve was sieved into 20-40 mesh particles after tableting, the loading amount was 2.0 g, the agent-oil ratio was 1.28, and the sample was analyzed after 900 seconds of reaction, and the material balance calculation was performed. The product distribution is shown in Table 1.
[0096] The following formula is used to calculate the micro-reverse conversion rate X of the raw material and the yield S of the product: i :
[0097]
[0098]
[0099]
[0100]
[0101] Table 1
[0102]
[0103] According to the data in Table 1, the iron-containing ZSM-5 molecular sieve prepared by the method of introducing peroxide in the present disclosure has a high relative crystallinity of about 80-87%. It can be seen from the transmission electron microscope photo of the iron-containing ZSM-5 molecular sieve prepared by Example 1 that the grain size of the iron-containing ZSM-5 molecular sieve prepared by the method of the present disclosure is 1-2μm; it can be seen from the STEM-Mapping photo of the iron-containing ZSM-5 molecular sieve prepared by Example 1 that the iron active components in the iron-containing ZSM-5 molecular sieve prepared by the method of the present disclosure are evenly distributed. It can be seen from the H2-TPR diagram of the iron-containing ZSM-5 molecular sieve prepared by Example 3 that the molecular sieve of Example 3 has no obvious peak within 100-700°C, indicating that the iron active components in the iron-containing ZSM-5 molecular sieve prepared by the method of the present disclosure are all present on the skeleton of the molecular sieve, and are not distributed on the outer surface of the molecular sieve. The H2-TPR diagram of the parent ZSM-5 molecular sieve prepared in comparative example D1 does not have an obvious peak within the range of 100-700°C because it does not contain iron species and there are no reducing species.
[0104] And according to the data in Tables 1 and 2, when the iron-containing ZSM-5 molecular sieve prepared by the method of the present invention is used for the catalytic cracking reaction of n-tetradecane and the catalytic cracking reaction of light hydrocarbons, a higher micro-reverse conversion rate and a better light olefin yield can be obtained; according to the comparison of Examples 1-3 and 5, when the molar ratio of the iron source, sodium persulfate and water in terms of Fe2O3 is preferably 1: (0.3-2.0): (200-800), the prepared catalyst can be used for the catalytic cracking of n-tetradecane to obtain a higher micro-reverse conversion rate and propylene yield; according to the comparison of Examples 1-3 and 5, When the sodium persulfate increases within a certain range, the crystallinity of the molecular sieve increases, and the prepared catalyst can be used for the catalytic cracking of n-tetradecane to obtain a higher micro-reverse conversion rate and a lower carbon olefin yield; according to Examples 3 and 6, when the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is preferably (35-90):1:(4-20):(500-1000), the prepared molecular sieve has a better catalytic cracking performance, and its use for the catalytic cracking of n-tetradecane can obtain a higher micro-reverse conversion rate and a lower carbon olefin yield.
[0105] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0106] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0107] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing an iron-containing ZSM-5 molecular sieve, the method comprising: S1, mixing a silicon source, an aluminum source, an alkali source, a seed crystal and water to obtain a first mixture; S2, mixing the iron source, peroxide, water and the first mixture and performing a hydrothermal reaction; Wherein, the peroxide is selected from one or more of sodium persulfate, hydrogen peroxide and Fenton's reagent.
2. The method according to claim 1, wherein: Step S2 includes: SS1. Mixing the iron source, peroxide and water to obtain a second mixture; the molar ratio of the iron source, peroxide and water in terms of Fe2O3 is 1:(0.2-2.5):(200-1400); preferably 1:(0.3-2.0):(200-800); SS2. The first mixture and the second mixture are mixed and then subjected to the hydrothermal reaction; the molar ratio of the first mixture calculated as Al2O3 to the second mixture calculated as Fe2O3 is 1:(0.01-3.0); preferably 1:(0.4-2.3).
3. The method according to claim 1, wherein: In step S1, the molar ratio of the silicon source calculated as SiO2, the aluminum source calculated as Al2O3, the alkali source calculated as alkali metal oxide and the water is (20-300):1:(2-30):(300-2500), preferably (35-60):1:(4-20):(500-1000); Calculated as SiO2, the amount of the seed crystal used is 5-15 wt%, preferably 7-12 wt%, relative to the total weight of the silicon source.
4. The method according to claim 1, wherein: In step S2, the conditions of the hydrothermal reaction include: temperature of 150-220° C. and time of 8-32 h.
5. The method according to claim 1, wherein: The method further comprises: subjecting the solid product obtained by the hydrothermal treatment to ammonium exchange and roasting treatment; the conditions of the roasting treatment include: temperature of 400-800° C., time of 0.5-8 hours, and atmosphere of air or water vapor.
6. The method according to claim 1, wherein: The silicon source includes one or more of silica gel, silicon dioxide, white carbon black and silicate; The aluminum source includes one or more of sodium metaaluminate, SB powder, aluminum alcoholate, aluminum oxide, aluminum hydroxide and aluminum sulfate; The alkali source includes sodium hydroxide and / or potassium hydroxide; The seed crystals include one or more ZSM-5 molecular sieves with a silicon-aluminum ratio of 20-50, and the average particle size of the ZSM-5 molecular sieve is 0.5-2 μm; The iron source is selected from one or more of ferric nitrate, ferric oxalate, ferric sulfate and ferric hydroxide.
7. The iron-containing ZSM-5 molecular sieve prepared by the method according to any one of claims 1 to 6.
8. The iron-containing ZSM-5 molecular sieve according to claim 7, wherein: The iron-containing ZSM-5 molecular sieve has a structure in which an iron active component is encapsulated inside the ZSM-5 molecular sieve; the iron active component is distributed on the framework of the ZSM-5 molecular sieve.
9. The iron-containing ZSM-5 molecular sieve according to claim 7, wherein: The specific surface area of the iron-containing ZSM-5 molecular sieve is 200-450m 2 / g, with a total pore volume of 0.130-0.24 cm 3 ·g -1 , the micropore volume is 0.100-0.20cm 3 ·g -1 , the mesopore volume is 0.010-0.10cm 3 ·g -1 , relative crystallinity is 80-100%; In the iron-containing ZSM-5 molecular sieve, the molar ratio of SiO2 to Al2O3 is 20-300; Relative to the total weight of the iron-containing ZSM-5 molecular sieve, the content of the iron active component calculated as Fe2O3 is 1-3% by weight.
10. Use of the iron-containing ZSM-5 molecular sieve according to any one of claims 7 to 9 in the catalytic cracking reaction of n-tetradecane.
11. The use according to claim 10, wherein: The conditions of the catalytic cracking reaction include: a temperature of 500-680°C, a reaction mass space velocity of 20-40h -1 , the reaction pressure is 0.8-1.2MPa, and the agent-oil weight ratio is 1-2.
Citation Information
Patent Citations
Low-cost green method for synthesizing Fe-ZSM-5 molecular sieve
CN105731492A
High-iron content Fe-ZSM-5 molecular sieve preparation method
CN108217681A
Method for synthesizing hierarchical porous Fe-ZSM-5 zeolite molecular sieve by crystal seed process
CN109721076A
Green energy-saving Fe-ZSM-5 molecular sieve synthesis method
CN110054199A
Metal modified mesoporous ZSM-5 molecular sieve and preparation method thereof