Graphdiyne-coated copper oxide one-dimensional nanowire with core-shell structure and preparation method thereof

By growing copper hydroxide nanowires on copper materials and converting them into copper oxide, combined with hexaethylbenzene catalysis, graphiteyne coated copper oxide one-dimensional nanowires were successfully prepared, solving the preparation problems in the prior art and realizing the material Improve performance and wide application.

CN119080050AInactive Publication Date: 2024-12-06NANTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191682.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prepare graphiteyne-coated copper oxide one-dimensional nanowires with core-shell structures, which limits their applications in the fields of energy storage, photoelectric sensors and electromagnetic shielding.

Method used

Copper hydroxide nanowires were grown by dilute hydrochloric acid treatment and alkaline persulfate solution reaction, and hexaethynylbenzene was used as a catalyst under low temperature conditions to gradually form graphiteyne nanosheets coated copper oxide nanowires. , realize the formation of core-shell structure.

Benefits of technology

The preparation of graphiteyne nanosheets uniformly coated copper oxide nanowires is realized, which enhances the electrochemical performance and photoelectric conversion ability of the material. The preparation method is simple, efficient, low energy consumption and wide applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080050A_ABST
    Figure CN119080050A_ABST
Patent Text Reader

Abstract

The invention discloses a graphdiyne-coated copper oxide one-dimensional nanowire with a core-shell structure and a preparation method of the graphdiyne-coated copper oxide one-dimensional nanowire. The graphdiyne-coated copper oxide one-dimensional nanowire is characterized in that the prepared one-dimensional nanowire has the core-shell structure, a core layer is a copper oxide nanowire, a shell layer is a graphdiyne nanosheet, and the graphdiyne nanosheet of the shell layer uniformly coats the surface of the copper oxide nanowire of the core layer. The preparation method of the one-dimensional nanowire comprises the following steps: growing a copper hydroxide one-dimensional nanowire on the surface of a copper substrate in situ; the preparation method comprises the following steps: taking a copper hydroxide nanowire as a core layer, providing a copper source as a catalyst, and growing a graphdiyne-coated nanosheet on the surface of the nanowire as a shell layer to obtain the graphdiyne-coated copper oxide one-dimensional nanowire with a core-shell structure. The preparation method provided by the invention is simple and efficient, the morphology of the prepared one-dimensional nanowire is controllable, the thicknesses of the core layer and the shell layer and the length of the nanowire can be accurately regulated and controlled, and a novel and reliable preparation way is provided for the graphdiyne heterojunction nano material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a graphyne-coated copper oxide one-dimensional nanowire with a core-shell structure, belonging to the technical field of nano material preparation. Background Art

[0002] One-dimensional semiconductor nanomaterials, such as nanotubes, nanowires, and nanobelts, have unique electronic, magnetic, and optical properties that are different from bulk materials due to their special structures and size effects. These unique properties make one-dimensional semiconductor nanomaterials have broad prospects in future applications such as optoelectronic devices, sensors, and electronic devices, and have become a hot topic in materials science and nanotechnology research. For example, as a representative of one-dimensional materials, the discovery of carbon nanotubes (CNTs) has opened up new horizons for the study of low-dimensional nanostructures. Subsequent one-dimensional semiconductor nanomaterials such as silicon (Si), gallium nitride (GaN), zinc sulfide (ZnS), zinc selenide (ZnSe) and other nanotube and nanowire heterojunctions have also attracted widespread attention from the scientific community. With the deepening of research, more and more scholars are committed to exploring the synthesis process, physical and chemical properties, and potential applications of one-dimensional semiconductor nanomaterials, for example, using more environmentally friendly and economical raw materials and methods to achieve large-scale production of one-dimensional semiconductor nanomaterials; exploring the performance optimization and multifunctional integration of nanomaterials to promote their application in high-performance electronic devices, optoelectronic devices, and biomedical fields.

[0003] Graphdiyne (GDY) is composed of sp and sp 2 A new type of carbon allotrope formed by hybridization, which is formed by conjugating benzene rings with 1,3-diyne bonds to form a two-dimensional planar network structure, with a large conjugated system, wide interplanar spacing, porosity, excellent chemical and thermal stability and semiconductor properties. Due to its special electronic structure and properties, it has excellent physical and chemical properties and shows potential application prospects in the fields of electronics, semiconductors, catalysis, etc. CN 114975920 A synthesized a core-shell structure graphyne coated with metal antimony as a negative electrode material for sodium ion batteries, which has excellent rate performance and long cycle performance, and excellent electrochemical performance. CN 116093278 A for the first time, a graphyne shell layer was grown in situ on the surface of a copper sulfide nano hollow cube at room temperature by a solvent method to obtain a negative electrode material for a sodium ion battery. Due to the improvement of the conductivity and ion diffusion performance of the material by the graphyne coating layer, and the alleviation of the volume expansion of the material during the charge and discharge process by the external coating layer and the hollow structure, it showed excellent cycle and rate performance. CN 117070189 A provides a core-shell structure nanowire containing hydrogenated graphene and a preparation method thereof, and proves that the nanowire can be used as an excellent wave absorbing material in the field of electromagnetic shielding.

[0004] Therefore, designing and preparing one-dimensional nanomaterials with a core-shell structure, constructing graphene / semiconductor heterojunctions, and exploring their electrochemical properties, photoelectric conversion capabilities, magnetic and wave absorption properties are of great practical significance for promoting the application of graphyne-based one-dimensional nanomaterials in energy storage, photoelectric sensors, electromagnetic shielding and other fields. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing graphyne-coated copper oxide one-dimensional nanowires with a core-shell structure.

[0006] 1. Growth of copper hydroxide nanowires

[0007] Prepare a 10wt% dilute hydrochloric acid solution, soak the copper substrate in the dilute hydrochloric acid for 10-30 minutes to remove oxides on the surface of the copper substrate, wash it with deionized water, and then vacuum dry it to obtain a pretreated copper substrate;

[0008] The pretreated copper substrate is immersed in an alkaline solution 1 of persulfate, and after standing for 10-60 minutes, the copper substrate is taken out, washed thoroughly with deionized water, and then vacuum dried to obtain a copper substrate coated with Cu(OH)2 one-dimensional nanowires, which is recorded as Cu(OH)2@Cu.

[0009] The copper substrate includes one of copper foil, copper wire / filament, copper mesh and copper sponge.

[0010] Persulfate is one or two of sodium persulfate, potassium persulfate and ammonium persulfate, with a concentration of 0.2-2.5 mol / L -1 .

[0011] The alkaline solution 1 is an aqueous solution of sodium hydroxide, potassium hydroxide, sodium carbonate, or sodium bicarbonate, with a concentration of 1.0-4.0 mol L -1 .

[0012] 2. Growth of GDY-coated Copper Oxide Nanowires with Core-Shell Structure

[0013] Cu(OH)2@Cu is added to polar solvent 2. At a temperature of 40-80°C, polar solvent 3 containing hexaethynylbenzene is slowly dropped into solution 2 containing Cu(OH)2@Cu. The reaction temperature is maintained and the reaction is carried out in the dark for 6-48 hours to obtain CuO@Cu wrapped by graphyne nanosheets, which is recorded as GDY@CuO@Cu.

[0014] Wherein, the polar solvent 2 is one or two of pyridine, N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, ethylene glycol dimethyl ether, dichloromethane, and 2-bromopyridine.

[0015] The polar solvent 3 is one or two of pyridine, N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, ethylene glycol dimethyl ether, dichloromethane, and 2-bromopyridine.

[0016] The concentration of hexaethynylbenzene in polar solvent 3 is 0.5-4.0mmol L -1 .

[0017] In summary, the method for preparing the core-shell structured graphyne-coated copper oxide one-dimensional nanowires of the present invention has the following advantages over the prior art:

[0018] 1. The present invention innovatively uses copper material as a substrate, in-situ grows copper hydroxide nanowires as a growth template for graphyne, and provides a copper source as a catalyst to obtain a one-dimensional nanowire material with a core-shell structure uniformly coated with graphyne nanosheets. The copper hydroxide nanowires serve as a core layer structure, and after being synchronously converted into copper oxide, they form a heterojunction with graphyne to enhance the material performance.

[0019] 2. The preparation method adopted by the present invention is simple and efficient. The growth of copper hydroxide nanowires is carried out at room temperature, and the growth of graphyne can be carried out at low temperature. The preparation method has low energy consumption, strong operability, and wide applicability, and can meet the actual needs of various industrial fields.

[0020] 3. The one-dimensional nanowires with a core-shell structure prepared in the present invention have controllable morphology, and can achieve precise regulation of the thickness of the core layer and the shell layer and the length of the nanowire by controlling the reaction conditions, thereby achieving performance regulation and optimization of the graphyne / copper oxide heterojunction nanomaterials. It has a wide range of applications and is simple and flexible to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a transmission electron microscope image of the graphyne-coated copper oxide one-dimensional nanowires obtained in Example 1. DETAILED DESCRIPTION

[0022] The preparation method of the Graphene-coated copper oxide one-dimensional nanowires with a core-shell structure of the present invention is further described below through specific examples.

[0023] Example 1

[0024] Prepare a 10wt% dilute hydrochloric acid solution, soak the copper mesh (150 mesh) in the dilute hydrochloric acid for 20 minutes to remove the oxide on the surface of the copper mesh, wash it with deionized water, and then vacuum dry it to obtain a pretreated copper mesh; soak the pretreated copper mesh in a sodium hydroxide aqueous solution of potassium persulfate, the potassium persulfate concentration being 1.3 mol L -1 , the concentration of sodium hydroxide is 2.5 mol L -1After the reaction was allowed to stand for 30 min, the copper mesh was taken out, washed with deionized water and dried in vacuo to obtain a copper mesh coated with Cu(OH)2 one-dimensional nanowires. Cu(OH)2@Cu was added to a pyridine solution containing hexaethynylbenzene (1.0 mmol L -1 ) was slowly added dropwise into the pyridine solution containing Cu(OH)2@Cu, the reaction temperature was maintained, and the reaction was carried out in the dark for 24 hours to obtain CuO@Cu wrapped by graphyne nanosheets.

[0025] Figure 1 This is a transmission electron microscope image of the graphyne-coated copper oxide one-dimensional nanowire with a core-shell structure obtained in this example. It can be seen from the image that the one-dimensional nanowire presents an obvious core-shell structure, the core layer is composed of copper oxide, and the shell layer is composed of graphyne nanosheets. The graphyne nanosheets are evenly distributed in the copper oxide nanowire.

[0026] Example 2

[0027] Prepare a 10wt% dilute hydrochloric acid solution, soak the copper mesh (300 mesh) in the dilute hydrochloric acid for 30 minutes to remove the oxide on the surface of the copper mesh, wash it with deionized water, and vacuum dry it to obtain a pretreated copper mesh; soak the pretreated copper mesh in a sodium hydroxide aqueous solution of potassium persulfate, the concentration of potassium persulfate is 2.0 mol L -1 , the concentration of sodium hydroxide is 3.0 mol L -1 After the reaction was allowed to stand for 30 min, the copper mesh was taken out, washed with deionized water and dried in vacuo to obtain a copper mesh coated with Cu(OH)2 one-dimensional nanowires. Cu(OH)2@Cu was added to a pyridine solution containing hexaethynylbenzene (1.0 mmol L -1 ) was slowly added dropwise into the pyridine solution containing Cu(OH)2@Cu, the reaction temperature was maintained, and the reaction was carried out in the dark for 24 hours to obtain CuO@Cu wrapped by graphyne nanosheets.

[0028] Example 3

[0029] Prepare a 10wt% dilute hydrochloric acid solution, soak the copper sponge in the dilute hydrochloric acid for 20 minutes to remove the oxide on the surface of the copper sponge, wash it with deionized water, and then vacuum dry it to obtain a pretreated copper sponge; soak the pretreated copper sponge in a sodium hydroxide aqueous solution of potassium persulfate, the concentration of potassium persulfate is 1.3 mol L -1 , the concentration of sodium hydroxide is 2.5 mol L -1 After the reaction was allowed to stand for 30 min, the copper sponge was taken out, washed with deionized water and dried in vacuo to obtain a copper sponge coated with Cu(OH)2 one-dimensional nanowires. Cu(OH)2@Cu was added to a pyridine solution containing hexaethynylbenzene (1.0 mmol L-1 ) was slowly added dropwise into the pyridine solution containing Cu(OH)2@Cu, the reaction temperature was maintained, and the reaction was carried out in the dark for 24 hours to obtain CuO@Cu wrapped by graphyne nanosheets.

[0030] Example 4

[0031] Prepare a 10wt% dilute hydrochloric acid solution, soak the copper sponge in the dilute hydrochloric acid for 20 minutes to remove the oxide on the surface of the copper sponge, wash it with deionized water, and then vacuum dry it to obtain a pretreated copper sponge; soak the pretreated copper sponge in a sodium hydroxide aqueous solution of potassium persulfate, the concentration of potassium persulfate is 1.3 mol L -1 , the concentration of sodium hydroxide is 2.5 mol L -1 After the reaction was allowed to stand for 30 min, the copper sponge was taken out, washed with deionized water and dried in vacuo to obtain a copper sponge coated with Cu(OH)2 one-dimensional nanowires. Cu(OH)2@Cu was added to a pyridine solution containing hexaethynylbenzene (1.0 mmol L -1 ) was slowly added dropwise to the pyridine solution containing Cu(OH)2@Cu, the reaction temperature was maintained, and the reaction was carried out in the dark for 48 hours to obtain CuO@Cu wrapped by graphyne nanosheets.

[0032] Example 5

[0033] Prepare a 10wt% dilute hydrochloric acid solution, soak the copper sponge in the dilute hydrochloric acid for 20 minutes to remove the oxide on the surface of the copper sponge, wash it with deionized water, and then vacuum dry it to obtain a pretreated copper sponge; soak the pretreated copper sponge in a potassium hydroxide aqueous solution of potassium persulfate, the concentration of potassium persulfate is 1.3 mol L -1 , the potassium hydroxide concentration is 2.5 mol L -1 After standing for 60 min, the copper sponge was taken out, washed with deionized water and dried in vacuo to obtain a copper sponge coated with Cu(OH)2 one-dimensional nanowires. Cu(OH)2@Cu was added to a pyridine solution at 60 °C. A pyridine solution containing hexaethynylbenzene (1.0 mmol L -1 ) was slowly added dropwise to the pyridine solution containing Cu(OH)2@Cu, the reaction temperature was maintained, and the reaction was carried out in the dark for 48 hours to obtain CuO@Cu wrapped by graphyne nanosheets.

Claims

1. A graphyne-coated copper oxide one-dimensional nanowire with a core-shell structure, characterized in that: The one-dimensional nanowire has a core-shell structure, the core layer is a copper oxide nanowire, the shell layer is a graphyne nanosheet, and the graphyne nanosheet of the shell layer is uniformly coated on the surface of the copper oxide nanowire of the core layer.

2. A method for preparing a core-shell structured graphyne-coated copper oxide one-dimensional nanowire, characterized in that: The following steps are involved: The copper substrate is pretreated by soaking in dilute hydrochloric acid for 10-30 minutes to remove oxides on the surface of the copper substrate, and the substrate is thoroughly washed with deionized water and then dried in a vacuum. The pretreated copper substrate is soaked in an alkaline solution 1 of persulfate, and the copper substrate is taken out after standing for 10-60 minutes, and then washed with deionized water and then dried in a vacuum to obtain a copper substrate coated with Cu(OH)2 one-dimensional nanowires, which is recorded as Cu(OH)2@Cu. Cu(OH)2@Cu is added to a polar solvent 2, and a polar solvent 3 containing hexaethynylbenzene is slowly added dropwise to the polar solvent 2 containing Cu(OH)2@Cu at a temperature of 40-80°C, and the reaction temperature is maintained and the reaction is carried out in the dark for 6-48 hours to obtain CuO@Cu coated with graphene nanosheets, which is recorded as GDY@CuO@Cu.

3. The method for preparing a one-dimensional copper oxide nanowire coated with graphyne having a core-shell structure as claimed in claim 2, characterized in that: The copper substrate includes one of copper foil, copper wire / filament, copper mesh and copper sponge.

4. The method for preparing a one-dimensional copper oxide nanowire coated with graphyne having a core-shell structure as claimed in claim 2, characterized in that: The persulfate is one or two of sodium persulfate, potassium persulfate and ammonium persulfate, with a concentration of 0.2-2.5 mol L -1 .

5. The method for preparing a one-dimensional copper oxide nanowire coated with graphyne having a core-shell structure as claimed in claim 2, characterized in that: The alkaline solution 1 is an aqueous solution of sodium hydroxide, potassium hydroxide, sodium carbonate, or sodium bicarbonate, with a concentration of 1.0-4.0 mol L -1 .

6. The method for preparing a one-dimensional copper oxide nanowire coated with graphyne having a core-shell structure as claimed in claim 2, characterized in that: The polar solvent 2 is one or two of pyridine, N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, ethylene glycol dimethyl ether, dichloromethane, and 2-bromopyridine.

7. The method for preparing a one-dimensional copper oxide nanowire coated with graphyne having a core-shell structure as claimed in claim 2, characterized in that: The polar solvent 3 is one or two of pyridine, N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, ethylene glycol dimethyl ether, dichloromethane, and 2-bromopyridine.

8. The method for preparing a one-dimensional copper oxide nanowire coated with graphyne having a core-shell structure as claimed in claim 2, characterized in that: The concentration of hexaethynylbenzene in the polar solvent 3 is 0.5-4.0 mmol L -1 .