Preparation method of sodium ferrous sulfate positive electrode material for sodium ion battery
In the preparation of sodium ferrous sulfate, sodium sulfate, mixed heating method of sodium sulfate, ferrous sulfate heptahydrate and triammonium citrate, the problems of complex and high cost in the existing technology are solved, and the preparation process is achieved. A low-cost, simple and efficient preparation method, the material exhibits good rate performance and cycle stability.
Patent Information
- Application Number
- CN202411244047.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
The preparation method of the existing sodium ion battery cathode material sodium ferrous sulfate is complex, has high cost, long synthesis cycle, and has harsh reaction conditions, making it difficult to be suitable for large-scale production.
Use sodium sulfate (Na2SO4) and ferrous sulfate heptahydrate (FeSO4.7H2O) at a molar ratio of 1:(1.25~2), add triammonium citrate (C6H5O7(NH4)3) to form a homogeneous solution, and then The heat was heated to 350°C at a temperature increase rate of 5°C/min under argon protection and insulated for 10 hours to prepare the sodium ferrous sulfate positive electrode material.
It realizes a low-cost, simple and efficient preparation process, suitable for large-scale production, the material has good rate performance and cycle stability, and is suitable as a positive electrode material for sodium ion battery.
Smart Images

Figure CN119080069A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a method for preparing a sodium ferrous sulfate positive electrode material for a sodium ion battery. Background Art
[0002] As a new type of sulfate polyanion sodium ion battery cathode material, sodium ferrous sulfate has a high working voltage (higher than 3.8 V vs. Na / Na + ), high energy density, low raw material cost, good structural stability and environmental friendliness, and is one of the positive electrode materials for sodium ion batteries with broad application prospects. At present, the commonly used preparation methods of sodium ferrous sulfate positive electrode materials (such as solid phase sintering method and hydrothermal method, etc.) have the disadvantages of complex process, long synthesis cycle, harsh reaction conditions and high process cost. To this end, the present invention proposes a new method for preparing sodium ferrous sulfate positive electrode materials for sodium ion batteries with low cost, simplicity and high efficiency. Summary of the invention
[0003] The object of the present invention is to provide a low-cost, simple and efficient method for preparing sodium ferrous sulfate positive electrode material for sodium ion batteries.
[0004] The specific steps are:
[0005] (1) Weigh sodium sulfate (Na2SO4) and FeSO4.7H2O in a molar ratio of 1:(1.25-2) and weigh a certain amount of ammonium citrate (C6H5O7(NH4)3) in an amount of 10% of the sum of the weights of Na2SO4 and FeSO4.7H2O.
[0006] (2) Mix the three substances (Na2SO4, FeSO4.7H2O and C6H5O7(NH4)3) weighed in step (1), and add a small amount of deionized water to the mixture to completely dissolve the mixture to form a homogeneous solution;
[0007] (3) The homogeneous solution obtained in step (2) is transferred to a porcelain boat, and the porcelain boat is placed in a tubular furnace protected by argon (> 99% Ar) and heated from room temperature to 350°C at a heating rate of 5°C / min, and kept at this temperature for 10 hours. The mixture is cooled to room temperature to obtain a sodium ferrous sulfate positive electrode material.
[0008] The advantages of the present invention are as follows: the method of the present invention has low preparation cost, is simple and efficient, and the preparation conditions are easy to control, and is suitable for large-scale production. The prepared sodium ferrous sulfate material has good rate performance and cycle stability as a positive electrode material for sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 This is the XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in Examples 1 to 4.
[0010] Figure 2 This is the SEM image of the sodium ferrous sulfate positive electrode material prepared in Example 2.
[0011] Figure 3 This is a rate performance diagram of the sodium ferrous sulfate positive electrode material prepared in Examples 1 to 4.
[0012] Figure 4 This is a cycle performance diagram of the sodium ferrous sulfate positive electrode material prepared in Examples 1 to 4. DETAILED DESCRIPTION
[0013] The present invention is further described below in conjunction with specific embodiments. It should be pointed out that the following embodiments are for those skilled in the art to better understand the present invention, rather than limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments based on the above content.
[0014] Embodiment 1:
[0015] (1) According to the molar ratio of sodium sulfate (Na2SO4) to ferrous sulfate heptahydrate (FeSO4.7H2O) of 1:1.25, weigh 0.284 g of Na2SO4 and 0.695 g of FeSO4.7H2O, and weigh 0.0979 g of triammonium citrate (C6H5O7(NH4)3) according to 10% of the sum of the weights of Na2SO4 and FeSO4.7H2O;
[0016] (2) Mix the three substances (Na2SO4, FeSO4.7H2O and C6H5O7(NH4)3) weighed in step (1), and add a small amount of deionized water to the mixture to completely dissolve the mixture to form a homogeneous solution;
[0017] (3) The homogeneous solution obtained in step (2) is transferred to a porcelain boat, and the porcelain boat is placed in a tubular furnace protected by argon (> 99% Ar) and heated from room temperature to 350°C at a heating rate of 5°C / min, and kept at this temperature for 10 hours. The mixture is cooled to room temperature to obtain a sodium ferrous sulfate positive electrode material.
[0018] Embodiment 2:
[0019] (1) According to the molar ratio of sodium sulfate (Na2SO4) to ferrous sulfate heptahydrate (FeSO4.7H2O) of 1:1.5, weigh 0.284 g of Na2SO4 and 0.834 g of FeSO4.7H2O, and weigh 0.1118 g of triammonium citrate (C6H5O7(NH4)3) according to 10% of the sum of the weights of Na2SO4 and FeSO4.7H2O;
[0020] (2) Mix the three substances (Na2SO4, FeSO4.7H2O and C6H5O7(NH4)3) weighed in step (1), and add a small amount of deionized water to the mixture to completely dissolve the mixture to form a homogeneous solution;
[0021] (3) The homogeneous solution obtained in step (2) is transferred to a porcelain boat, and the porcelain boat is placed in a tubular furnace protected by argon (> 99% Ar) and heated from room temperature to 350°C at a heating rate of 5°C / min, and kept at this temperature for 10 hours. The mixture is cooled to room temperature to obtain a sodium ferrous sulfate positive electrode material.
[0022] Embodiment 3:
[0023] (1) According to the molar ratio of sodium sulfate (Na2SO4) to ferrous sulfate heptahydrate (FeSO4.7H2O) of 1:1.75, weigh 0.284 g of Na2SO4 and 0.973 g of FeSO4.7H2O, respectively, and weigh 0.1257 g of triammonium citrate (C6H5O7(NH4)3) according to 10% of the sum of the weights of Na2SO4 and FeSO4.7H2O;
[0024] (2) Mix the three substances (Na2SO4, FeSO4.7H2O and C6H5O7(NH4)3) weighed in step (1), and add a small amount of deionized water to the mixture to completely dissolve the mixture to form a homogeneous solution;
[0025] (3) The homogeneous solution obtained in step (2) is transferred to a porcelain boat, and the porcelain boat is placed in a tubular furnace protected by argon (> 99% Ar) and heated from room temperature to 350°C at a heating rate of 5°C / min, and kept at this temperature for 10 hours. The mixture is cooled to room temperature to obtain a sodium ferrous sulfate positive electrode material.
[0026] Embodiment 4:
[0027] (1) According to the molar ratio of sodium sulfate (Na2SO4) to ferrous sulfate heptahydrate (FeSO4.7H2O) of 1:2, weigh 0.284 g of Na2SO4 and 1.112 g of FeSO4.7H2O, and weigh 0.1396 g of triammonium citrate (C6H5O7(NH4)3) according to 10% of the sum of the weights of Na2SO4 and FeSO4.7H2O;
[0028] (2) Mix the three substances (Na2SO4, FeSO4.7H2O and C6H5O7(NH4)3) weighed in step (1), and add a small amount of deionized water to the mixture to completely dissolve the mixture to form a homogeneous solution;
[0029] (3) The homogeneous solution obtained in step (2) is transferred to a porcelain boat, and the porcelain boat is placed in a tubular furnace protected by argon (> 99% Ar) and heated from room temperature to 350°C at a heating rate of 5°C / min, and kept at this temperature for 10 hours. The mixture is cooled to room temperature to obtain a sodium ferrous sulfate positive electrode material.
[0030] The auxiliary agent C6H5O7(NH4)3) used in Examples 1 to 4 is only an example to enable those skilled in the art to better understand the present invention, but does not impose any limitation on the present invention.
[0031] Electrochemical performance test: The sodium ferrous sulfate material prepared in the example was used as the active material, the conductive carbon black (Super P) was used as the conductive agent, and the polyvinylidene fluoride (PVDF) was used as the binder. After being mixed and ground evenly in a mass ratio of 7:2:1, an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, and the mixture was evenly coated on an aluminum foil after being mixed into a slurry. The mixture was vacuum dried at 80 °C for 12 hours, and the electrode sheet was obtained after punching. The electrode sheet obtained after punching was used as the working electrode, the metal sodium sheet was used as the counter electrode, the glass fiber was used as the diaphragm, and 1 mol L -1 NaClO4 was dissolved in a 1:1 volume ratio of ethylene carbonate and diethyl carbonate solution and a 5% by mass fluoroethylene carbonate solution was added as the electrolyte. The CR2025 button cell was assembled in an argon-filled glove box. The constant current charge and discharge performance of the battery was tested using a BTS-5V / 10 mA charge and discharge tester from Shenzhen Xinwei Company. The charge and discharge voltage range was 2-4.5 V, and the current density during the cycle performance test was 0.05 A g -1 The current density of the rate performance test was 0.01 A g -1 , 0.02 A g -1 , 0.05 A g -1 , 0.1 A g -1 , 0.2 A g -1, 0.5 A g -1 and 0.01 A g -1 The sodium storage performance test results of the samples prepared in all Examples 1 to 4 are listed in Table 1 and Table 2.
[0032] Table 1: Rate performance test results of samples prepared in Examples 1 to 4
[0033]
[0034] Table 2: Cyclic performance test results of samples prepared in Examples 1 to 4
[0035]
[0036] like Figure 1 As shown, it is the XRD spectrum of the sodium ferrous sulfate positive electrode material prepared in Examples 1 to 4. It can be seen from the figure that the main phase of the material prepared by the present invention is sodium ferrous sulfate (Na 2.5 Fe 1.75 (SO4)3), the material has no obvious impurity phase generation.
[0037] like Figure 2 , which is a SEM image of the sodium ferrous sulfate positive electrode material prepared in Example 2. As can be seen from the figure, there are many holes on the surface of the sodium ferrous sulfate positive electrode material prepared in the present invention.
[0038] like Figure 3 As shown, the sodium ferrous sulfate positive electrode materials prepared in Examples 1 to 4 were subjected to different current densities (0.01, 0.02, 0.05, 0.1, 0.2, 0.5, 0.01 A g -1 ) under the rate performance curve. It can be seen from the figure that the sodium ferrous sulfate positive electrode material prepared in Example 2 has a relatively better rate performance. -1 The current density is still 66 mAh g -1 The discharge capacity.
[0039] like Figure 4 As shown, the sodium ferrous sulfate positive electrode material prepared in Examples 1 to 4 is 0.05 A g -1 Cyclic performance curve under current density. It can be seen from the figure that the sodium ferrous sulfate positive electrode material prepared in Example 2 has good cycle stability. -1 After 100 cycles at the same current density, the discharge capacity remains at 76 mAh g -1 .
Claims
1. A method for preparing a sodium ferrous sulfate positive electrode material for a sodium ion battery, characterized in that: The specific steps are: (1) Weigh sodium sulfate (Na2SO4) and FeSO4.7H2O in a molar ratio of 1:(1.25-2) respectively, and weigh a certain amount of triammonium citrate (C6H5O7(NH4)3) in an amount of 10% of the sum of the weights of the weighed Na2SO4 and FeSO4.7H2O; (2) Mix the three substances (Na2SO4, FeSO4.7H2O and C6H5O7(NH4)3) weighed in step (1), and add a small amount of deionized water to the mixture to completely dissolve the mixture to form a homogeneous solution; (3) The homogeneous solution obtained in step (2) is transferred to a porcelain boat, and the porcelain boat is placed in a tubular furnace protected by argon (> 99% Ar) and heated from room temperature to 350°C at a heating rate of 5°C / min, and kept at this temperature for 10 hours. The mixture is cooled to room temperature to obtain a sodium ferrous sulfate positive electrode material.