Preparation method of stable polyferric sulfate
By replacing the traditional nitric acid catalyst with zirconium-loaded alumina-based composite catalyst, the problems of poor polymeric iron sulfate treatment effect and poor stability are solved, and the preparation of polymeric iron sulfate with higher purity and stability is achieved, which significantly improves the preparation of polymeric iron sulfate The water treatment effect is reduced and the insoluble substance generation is reduced.
Patent Information
- Application Number
- CN202411192083.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The water treatment effect of polymerized iron sulfate is not ideal and the finished product is poorly stable, mainly because the residue of sodium nitrate caused by the traditional nitric acid catalyst used in the oxygen oxidation method affects the purity and stability of the product.
Alumina-based composite catalyst supported by zirconium cerium is used to replace the traditional nitric acid catalyst. The catalytic oxidation reaction is carried out by adding concentrated sulfuric acid, ferrous sulfate, and alumina-based composite catalyst supported by zirconium cerium to water to obtain a stable polymerized iron sulfate.
The purity and stability of polymerized iron sulfate are improved, and the water treatment effect is better. After 180 days of placement, the content of insoluble matter has not increased significantly. The amount of catalyst is saved without changing the production process and efficiency.
Smart Images

Figure CN119080073A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic polymer chemistry, and in particular to a method for preparing stable polyferric sulfate. Background Art
[0002] New, high-quality, high-efficiency iron salt inorganic polymer flocculant, mainly used for water purification, excellent effect, good water quality, does not contain harmful substances such as aluminum, chlorine and heavy metal ions, and no water transfer of iron ions, non-toxic, harmless, safe and reliable, deturbidity removal, decolorization, deoiling, dehydration, sterilization, deodorization, algae removal, removal of COD, BOD and heavy metal ions in water, etc. It is also used for industrial wastewater treatment, such as printing and dyeing wastewater, etc., and is also widely used in casting, papermaking, medicine, leather making, etc.
[0003] Polyferric sulfate (PFS) is a highly efficient inorganic polymer flocculant, which is widely used in the field of water treatment. At present, the domestic production capacity of polyferric sulfate has reached 3 million tons, and it is one of the major exporters of polyferric sulfate in the world. The main processes for producing polyferric sulfate include oxygen oxidation, oxidant oxidation, microbial oxidation, etc. Among them, oxygen oxidation is the most widely used. However, the oxygen oxidation process requires a large amount of chemicals such as sodium nitrite or nitric acid as co-catalysts, which will lead to a certain amount of sodium nitrate in the finished product, which will not only affect the application effect of the water treatment agent but also affect the stability of the finished water treatment agent. Summary of the invention
[0004] In order to solve the technical problems of unsatisfactory water treatment effect of polyferric sulfate and poor stability of finished product, a method for preparing stable polyferric sulfate is provided. The polyferric sulfate product prepared by the present invention using a zirconium-cerium loaded alumina-based composite catalyst to replace the traditional nitric acid catalyst has the advantages of higher purity, better stability and better water treatment effect.
[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:
[0006] A method for preparing stable polyferric sulfate comprises the following steps:
[0007] Concentrated sulfuric acid, ferrous sulfate, and zirconium-cerium loaded alumina-based composite catalyst are sequentially added to water, stirred evenly, and then transferred to a reactor, oxygen is introduced, and a catalytic oxidation reaction is performed until the ferrous content in the system is less than 0.01wt%, and the solid-liquid separation and recovery of the solid composite catalyst are performed to obtain a stable polyferric sulfate;
[0008] In the composite catalyst, the total mass of zirconium element and cerium element accounts for 10-30% of the composite catalyst.
[0009] Furthermore, in the composite catalyst, the mass ratio of zirconium element to cerium element is 0.6-0.8:0.2-0.4.
[0010] Furthermore, the method for obtaining the composite catalyst is: under stirring conditions, adding alumina microspheres to a solution containing zirconium salt and cerium salt, dissolving and dispersing them evenly to form a mixed solution, adding ammonia water dropwise, adjusting the pH value of the system to 8-11, so that zirconium ions and cerium ions co-precipitate on the alumina microspheres, separating the solid and liquid, drying, and calcining to obtain the alumina-based composite catalyst loaded with zirconium and cerium.
[0011] Further, in the mixed solution, the mass percentage of the alumina microspheres is 5-15%, the mass percentage of the zirconium salt is 2%-20%, the mass percentage of the cerium salt is 1%-10%, and the balance is the solvent; preferably, in the mixed solution, the mass percentage of the alumina microspheres is 6-10%, the mass percentage of the zirconium salt is 3%-10%, the mass percentage of the cerium salt is 1%-6%, and the balance is the solvent;
[0012] The mass percentage of the ammonia water is 5-15%;
[0013] The calcination temperature is 400-600° C. and the calcination time is 1.5-3.0 hours.
[0014] Furthermore, the mass percentage of the concentrated sulfuric acid is more than 80%; the ferrous content in the ferrous sulfate is at least 13.5wt%; the time of the catalytic oxidation reaction is 50-90min, and no additional heat source is required during the reaction process.
[0015] Furthermore, the mass ratio of the concentrated sulfuric acid, the ferrous sulfate, water, and the oxygen introduced is 0.08-0.12:1.1-1.2:0.5-0.55:0.2-0.3; calculated based on the amount of polyferric sulfate produced, the amount of the composite catalyst used is 1-3% of the total iron mass of the polyferric sulfate produced.
[0016] Beneficial technical effects:
[0017] The present invention adopts a zirconium-cerium loaded alumina-based composite catalyst to replace a traditional sodium nitrite or nitric acid catalyst to prepare polyferric sulfate without changing the production process device and the production efficiency. Not only can the obtained polyferric sulfate product be purer and have a better water treatment effect, but its own stability is also greatly improved. After being placed for 180 days, the insoluble matter content therein does not increase significantly. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The figure is a comparison chart of the stability performance of the polyferric sulfate prepared by the methods of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0020] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.
[0021] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.
[0022] The particle size of the alumina microspheres used in the following preparation examples is 2.0±0.05 mm.
[0023] Prepared 1
[0024] Preparation of alumina-based composite catalyst loaded with zirconium and cerium:
[0025] Under stirring conditions, 7.25g of zirconium nitrate and 3.25g of cerium nitrate were dissolved in 100mL of water, and 10g of alumina microspheres were added. After dissolution and dispersion to form a mixed solution, 8% ammonia water was added dropwise to the mixed solution until the pH value of the system was 9.81, so that zirconium ions and cerium ions were co-precipitated on the alumina microspheres. After solid-liquid separation and drying, the mixture was calcined at 500°C for 2.0h to obtain an alumina-based composite catalyst loaded with zirconium and cerium.
[0026] In the composite catalyst of this case, the total mass of zirconium element and cerium element accounts for 30wt% of the composite catalyst, wherein the mass ratio of zirconium to cerium is 0.65:0.35.
[0027] Preparation Example 2
[0028] Preparation of alumina-based composite catalyst loaded with zirconium and cerium:
[0029] Under stirring conditions, 3.90g of zirconium nitrate and 1.40g of cerium nitrate were dissolved in 100mL of water, and 10g of alumina microspheres were added. After dissolution and dispersion to form a mixed solution, 10% ammonia water was added dropwise until the pH value of the system was 9.69, so that zirconium ions and cerium ions were co-precipitated on the alumina microspheres. After solid-liquid separation and drying, the mixture was calcined at 500°C for 2.2h to obtain an alumina-based composite catalyst loaded with zirconium and cerium.
[0030] In the composite catalyst of this case, the total mass of zirconium and cerium elements accounts for 15wt% of the composite catalyst, wherein the mass ratio of zirconium to cerium is 0.7:0.3.
[0031] Preparation Example 3
[0032] Preparation of alumina-based composite catalyst loaded with zirconium and cerium:
[0033] Under stirring conditions, 6.97g of zirconium nitrate and 1.94g of cerium nitrate were dissolved in 100mL of water, and 10g of alumina microspheres were added. After dissolution and dispersion to form a mixed solution, 12% ammonia water was added dropwise to the system pH = 9.90 to allow zirconium ions and cerium ions to co-precipitate on the alumina microspheres. After solid-liquid separation and drying, the mixture was calcined at 500°C for 2.5h to obtain an alumina-based composite catalyst loaded with zirconium and cerium.
[0034] In the composite catalyst of this case, the total mass of zirconium element and cerium element accounts for 25wt% of the composite catalyst, wherein the mass ratio of zirconium to cerium is 0.75:0.25.
[0035] Example 1
[0036] A method for preparing stable polyferric sulfate comprises the following steps:
[0037] In a 1000mL beaker, 150g of water was added, followed by 30g of concentrated sulfuric acid (98% by mass) and 330g of ferrous sulfate (18% by mass of ferrous ions). After stirring, 0.89g of the composite catalyst of Preparation Example 1 was added (1.5% of the total iron mass of the produced polyferric sulfate), and stirring was continued. The mixture was then transferred to a 1L pressure-resistant reactor, 15g of oxygen was introduced, and a catalytic oxidation reaction was carried out for 80min until the ferrous content in the system was less than 0.01wt%. The solid-liquid separation was performed to recover the solid composite catalyst of Preparation Example 1 (it can be activated before being put into use. Since the composite catalyst has a large particle size, it can be directly separated by a mesh bag), and liquid stable polyferric sulfate was obtained.
[0038] The polyferric sulfate prepared in this case was tested, and the total iron content of the product was 11.31% by mass, and the basicity was 12.5%. The polyferric sulfate prepared in this case was recorded as PFS-1.
[0039] Example 2
[0040] A method for preparing stable polyferric sulfate comprises the following steps:
[0041] In a 1000mL beaker, 150g of water was added, followed by 30g of concentrated sulfuric acid (98% by mass) and 330g of ferrous sulfate (18% by mass of ferrous ions). After stirring, 0.89g of the composite catalyst of Preparation Example 2 was added (1.5% of the total iron mass of the produced polyferric sulfate), and stirring was continued. The mixture was then transferred to a 1L pressure-resistant reactor, 15g of oxygen was introduced, and a catalytic oxidation reaction was carried out for 65min until the ferrous content in the system was less than 0.01wt%. The solid-liquid separation was performed to recover the composite catalyst of Preparation Example 1 in the solid state (it can be activated before being put into use. Since the composite catalyst has a large particle size, it can be directly separated by a mesh bag), thereby obtaining a liquid stable polyferric sulfate.
[0042] The polyferric sulfate prepared in this case was tested, and the total iron content of the product was 11.30% by mass, and the basicity was 12.3%. The polyferric sulfate prepared in this case was recorded as PFS-2.
[0043] Example 3
[0044] A method for preparing stable polyferric sulfate comprises the following steps:
[0045] In a 1000mL beaker, 150g of water was added, followed by 30g of concentrated sulfuric acid (98% by mass) and 330g of ferrous sulfate (18% by mass of ferrous ions). After stirring, 0.89g of the composite catalyst of Preparation Example 3 was added (1.5% of the total iron mass of the produced polyferric sulfate), and stirring was continued. The mixture was then transferred to a 1L pressure-resistant reactor, 15g of oxygen was introduced, and a catalytic oxidation reaction was carried out for 60min until the ferrous content in the system was less than 0.01wt%. The solid-liquid separation was performed to recover the composite catalyst of Preparation Example 1 (which can be activated before use. Since the composite catalyst has a large particle size, it can be directly separated by a mesh bag), and liquid stable polyferric sulfate was obtained.
[0046] The polyferric sulfate prepared in this case was tested, and the total iron content of the product was 11.29% by mass, and the basicity was 12.3%. The polyferric sulfate prepared in this case was recorded as PFS-3.
[0047] Comparative Example 1
[0048] Add 150g of water to a 1000mL beaker, then add 30g of concentrated sulfuric acid (98% by mass), and finally add 330g of ferrous sulfate (18% by mass fraction of ferrous ions), stir evenly, transfer to a 1L pressure reactor, add 5g of sodium nitrite, introduce 15g of oxygen, and react for 75min until the ferrous content in the system is less than 0.01wt%, to obtain liquid polyferric sulfate, at which time the total iron mass percentage of the obtained polyferric sulfate is 11.21%, and the basicity is 11.9%. The polyferric sulfate obtained in this case is recorded as PFS-4.
[0049] Comparative Example 2
[0050] Aluminum oxide as a catalyst cannot catalyze the reaction to obtain polyferric sulfate.
[0051] Comparative Example 3
[0052] The composite catalyst only loaded zirconium, and the proportion of zirconium was the same as the total proportion of zirconium and cerium in Preparation Example 1. Polyferric sulfate was prepared by the method of Example 1 using the composite catalyst only loaded with zirconium.
[0053] The total iron content of the polyferric sulfate is 11.26% by mass, and the basicity is 11.96%. The polyferric sulfate prepared in this case is recorded as PFS-5.
[0054] Comparative Example 4
[0055] The composite catalyst only loaded cerium, and the proportion of cerium was the same as the total proportion of zirconium and cerium in Preparation Example 1. Polyferric sulfate was prepared by the method of Example 1 using the composite catalyst only loaded with zirconium.
[0056] The total iron content of the polyferric sulfate is 11.30% by mass, and the basicity is 12.03%. The polyferric sulfate prepared in this case is recorded as PFS-6.
[0057] By comparing the above production processes, it can be seen that after using the zirconium-cerium loaded alumina-based composite catalyst, the production efficiency of the same proportion of raw materials has been improved to a certain extent.
[0058] The above products were used for water treatment and the coagulation performance of each product was compared. The results are shown in Table 1.
[0059] Table 1 Comparison of coagulation performance of products in various cases
[0060]
[0061] (Note: raw water turbidity is 50NTU, pH=7.23, water temperature is 15℃)
[0062] As can be seen from Table 1, the polyferric sulfate prepared by the composite catalyst has excellent turbidity removal performance under the same dosage condition. Compared with samples PSF-5 and PFS-6 prepared by a single metal-loaded catalyst, the dosage of the bimetallic-loaded composite catalyst of the present invention can save at least 25% of the dosage.
[0063] The stability of the products of Example 1 and Comparative Example 1 was compared. The test method was carried out according to the method 5.7 in GB / T14591-216. The stability performance comparison of the two products is shown in Figure 1 .Depend on Figure 1 It can be seen that within 180 days of placement, the insoluble matter of PFS-1 was between 0.04% and 0.06%, while the insoluble matter of PFS-4 increased from 0.05% to 0.62%, which indicates that PFS-4 prepared by the method of Comparative Example 1 was severely hydrolyzed and had poor stability. However, the polyferric sulfate prepared by the method of the present invention has good stability and is not prone to hydrolysis.
[0064] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing stable polyferric sulfate, characterized in that: The steps include: Concentrated sulfuric acid, ferrous sulfate, and zirconium-cerium loaded alumina-based composite catalyst are sequentially added to water, stirred evenly, and then transferred to a reactor, oxygen is introduced, and a catalytic oxidation reaction is performed until the ferrous content in the system is less than 0.01wt%, and the solid-liquid separation and recovery of the solid composite catalyst are performed to obtain a stable polyferric sulfate; In the composite catalyst, the total mass of zirconium element and cerium element accounts for 10-30% of the composite catalyst.
2. The method for preparing a stable polyferric sulfate according to claim 1, characterized in that: In the composite catalyst, the mass ratio of zirconium element to cerium element is 0.6-0.8:0.2-0.
4.
3. The method for preparing a stable polyferric sulfate according to claim 2, characterized in that: The method for obtaining the composite catalyst is as follows: under stirring conditions, alumina microspheres are added to a solution containing zirconium salt and cerium salt, after dissolving and dispersing uniformly to form a mixed solution, ammonia water is added dropwise, and the pH value of the system is adjusted to 8-11, so that zirconium ions and cerium ions are co-precipitated on the alumina microspheres, and after solid-liquid separation and drying, calcination is performed to obtain the alumina-based composite catalyst loaded with zirconium and cerium.
4. The method for preparing a stable polyferric sulfate according to claim 3, characterized in that: In the mixed solution, the mass percentage of the alumina microspheres is 5-15%, the mass percentage of the zirconium salt is 2%-20%, the mass percentage of the cerium salt is 1%-10%, and the balance is solvent; The mass percentage of the ammonia water is 5-15%; The calcination temperature is 400-600° C. and the calcination time is 1.5-3.0 hours.
5. The method for preparing a stable polyferric sulfate according to claim 1, characterized in that: The mass percentage of the concentrated sulfuric acid is more than 80%; the ferrous content in the ferrous sulfate is at least 13.5wt%; and the time of the catalytic oxidation reaction is 50-90min.
6. The method for preparing a stable polyferric sulfate according to claim 5, characterized in that: The mass ratio of the concentrated sulfuric acid, the ferrous sulfate, water and the oxygen introduced is 0.08-0.12:1.1-1.2:0.5-0.55:0.2-0.3; calculated based on the amount of polyferric sulfate produced, the amount of the composite catalyst used is 1-3% of the total iron mass of the polyferric sulfate produced.