Cement reinforcing agent as well as preparation method and application thereof

By using raw materials such as triethanolamine and silica sol to form a cement reinforcement with a mesh macromolecular structure, the existing cement reinforcement has been solved, and the compressive strength and stability of the cement is significantly improved, effectively inhibiting the pressure resistance of the cement. The migration of chloride ions extends the service life of concrete.

CN119080433APending Publication Date: 2024-12-06SHANDONG ZHONGYAN BUILDING MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411234245.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing cement reinforcement has limited effect in improving the strength of concrete and is insufficiently adaptable to different aggregates, which may lead to corrosion of steel bars and salt erosion, affecting the durability of concrete.

Method used

The cement reinforcement agent with a network macromolecular structure is formed by using triethanolamine, silica sol, silane coupling agent, citric acid and other raw materials. The modified silica sol combines with triethanolamine and citric acid to improve the cement base. The mechanical properties of the material and inhibit the migration of chloride ions.

Benefits of technology

It significantly improves the compressive strength and stability of cement, effectively blocks the migration of chloride ions, and extends the service life of concrete.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of cement-based building material admixtures, in particular to a cement reinforcing agent and a preparation method and application thereof.The cement reinforcing agent with a net-shaped macromolecular structure is prepared from triethanolamine, diethylene glycol, silica sol, a silane coupling agent, water, ethyl alcohol, citric acid and a dispersing agent. The mechanical property of the cement-based material is improved, and chloride ion migration is effectively inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement-based building material admixtures, and in particular to a cement reinforcing agent and a preparation method and application thereof. Background Art

[0002] With the improvement of infrastructure engineering technology, the performance requirements for the bulk building materials used have increased accordingly. As the requirements of engineering construction continue to develop towards high strength and high durability, adding cement enhancers to cement-based building materials is a commonly used technical measure.

[0003] At present, the cement enhancers used in the market are mainly divided into organic and inorganic types. Inorganic types mainly include nitrates, sulfates, chlorides, etc. Although they have early strength enhancement effects, they may cause steel corrosion and salt erosion, affecting the durability of concrete. Organic types often add triethanolamine and diethyl monoisopropanolamine as enhancers to improve the strength of concrete, but the effect of additives is limited, and the strengthening effect is not stable enough, and there are limitations on the adaptability to different aggregates.

[0004] Silicon dioxide is usually crystalline in nature, while silicon dioxide nanoparticles artificially synthesized by sol-gel, hydrothermal, template agent and other methods are usually amorphous, called silica sol. Silica sol is widely used in many high-end fields such as aerospace, catalyst carrier, targeted drug delivery, etc. With the continuous improvement of silica sol production technology, the cost has been greatly reduced and it is often used in civil buildings. Summary of the invention

[0005] In order to overcome the problems existing in the prior art, the present invention provides a cement strengthener, which uses triethanolamine, diethylene glycol, silica sol, silane coupling agent, water, ethanol, citric acid and dispersant as raw materials to prepare a cement strengthener with a network macromolecular structure, which can stimulate cement strength, improve the mechanical properties of cement-based materials and effectively inhibit chloride ion migration.

[0006] Specifically, the preparation method of the cement reinforcing agent of the present invention comprises the following steps:

[0007] 1) Weigh 20-40 parts of triethanolamine, 20-40 parts of diethylene glycol, 5-10 parts of silica sol, 3-5 parts of silane coupling agent, 1-5 parts of water, 15-25 parts of ethanol, 1-3 parts of citric acid, and 0.3-1 parts of dispersant by weight.

[0008] 2) Mix the silane coupling agent, water and ethanol evenly and stir to obtain a hydrolyzate.

[0009] 3) Mix the hydrolyzate and silica sol to obtain liquid A.

[0010] 4) Mix triethanolamine, diethylene glycol and dispersant, add citric acid, mix well to obtain liquid B.

[0011] 5) Heat liquid A and liquid B, mix, and stir while keeping warm to obtain.

[0012] Preferably, the silica sol is neutral silica sol.

[0013] Preferably, the silane coupling agent is at least one of KH550, KH560, and KH570. More preferably, the silane coupling agent is KH550, which is hydrolyzed in the environment of step 2), and the ethoxy group (-C2H5O) contained in the coupling agent reacts with water to transform into a silanol (-Si-OH) functional group, which can undergo dehydration condensation with the silanol on the nano-SiO2, thereby achieving the purpose of modification.

[0014] Preferably, the ethanol is anhydrous ethanol.

[0015] Preferably, the dispersant is at least one of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.

[0016] Preferably, the stirring time in step 2) is 3-5 h.

[0017] Preferably, in step 5), the mixture is heated to 70-85° C. and stirred for 30-60 min.

[0018] The present invention also relates to a cement reinforcing agent, which is specifically prepared by the above-mentioned preparation method.

[0019] The present invention also relates to the use of the above cement reinforcing agent in cement-based building materials. Preferably, the amount of the cement-based reinforcing agent added is 0.3-1% of the mass of the cementitious material.

[0020] Nano silicon dioxide, triethanolamine and diethylene glycol in the silica sol of the present invention are coupled with a silane coupling agent to obtain a macromolecular reinforcing agent containing a silica sol component. After the silica sol is modified by the silane coupling agent, it can form a network macromolecular structure with triethanolamine and diethylene glycol modified by citric acid, and improve the hydration density of cement-based materials, and can effectively block the migration of chloride ions in cement, thereby improving the stability and strength of cement. DETAILED DESCRIPTION

[0021] In order to prove the technical effect of the present invention, a cement enhancer was prepared and its use effect was tested. During the test, neutral silica sol was selected as silica sol, KH550 was selected as silane coupling agent, anhydrous ethanol was selected as ethanol, the test specimen was prepared by standard mortar test, P·O42.5 cement was used as cement, the standard mortar ratio was 450g cement, 1350g standard sand, 225g water, the amount of cement enhancer added was 0.6% of the mass of the cementitious material, and the blank mortar specimen without adding cement enhancer had a 3d compressive strength of 19.3MPa, a 7d compressive strength of 24.5MPa, a 28d compressive strength of 42.7MPa, and a chloride ion diffusion coefficient of 20.2×10 - 12 m 2 / s.

[0022] Example 1

[0023] The cement reinforcing agent, the preparation method comprises the following steps:

[0024] 1) Weigh 35 parts of triethanolamine, 30 parts of diethylene glycol, 8 parts of silica sol, 4 parts of silane coupling agent, 4 parts of water, 22 parts of ethanol, 3 parts of citric acid, and 0.5 parts of sodium hexametaphosphate by weight.

[0025] 2) Mix the silane coupling agent, water and ethanol evenly and stir for 4 hours to obtain a hydrolyzate.

[0026] 3) Mix the hydrolyzate and silica sol to obtain liquid A.

[0027] 4) Mix triethanolamine, diethylene glycol and sodium hexametaphosphate, add citric acid, mix well to obtain liquid B.

[0028] 5) Heat liquid A and liquid B to 75°C, mix, and stir at this temperature for 30 minutes.

[0029] The test results show that the 3d compressive strength of the mortar is 23.6MPa, the 7d compressive strength is 29.8MPa, the 28d compressive strength is 49.1MPa, and the chloride ion diffusion coefficient is 5.2×10 -12 m 2 / s.

[0030] Example 2

[0031] The cement reinforcing agent, the preparation method comprises the following steps:

[0032] 1) Weigh 40 parts of triethanolamine, 35 parts of diethylene glycol, 5 parts of silica sol, 3 parts of silane coupling agent, 2 parts of water, 15 parts of ethanol, 2 parts of citric acid, and 0.6 parts of sodium tripolyphosphate by weight.

[0033] 2) Mix the silane coupling agent, water and ethanol evenly and stir for 4 hours to obtain a hydrolyzate.

[0034] 3) Mix the hydrolyzate and silica sol to obtain liquid A.

[0035] 4) Mix triethanolamine, diethylene glycol and sodium tripolyphosphate, add citric acid, mix well to obtain liquid B.

[0036] 5) Heat liquid A and liquid B to 75°C, mix, and stir at this temperature for 30 minutes.

[0037] The test results show that the 3d compressive strength of the mortar is 23.0MPa, the 7d compressive strength is 28.7MPa, the 28d compressive strength is 48.5MPa, and the chloride ion diffusion coefficient is 6.1×10 -12 m 2 / s.

[0038] Comparative Example 1

[0039] The cement reinforcing agent, the preparation method comprises the following steps:

[0040] 1) Weigh 40 parts of triethanolamine, 35 parts of diethylene glycol, 4 parts of silane coupling agent, 4 parts of water, 22 parts of ethanol, 3 parts of citric acid, and 0.5 parts of sodium hexametaphosphate by weight.

[0041] 2) Mix the silane coupling agent, water and ethanol evenly and stir for 4 hours to obtain a hydrolyzate.

[0042] 3) Mix triethanolamine, diethylene glycol and sodium hexametaphosphate, add citric acid, mix well to obtain liquid B.

[0043] 4) Heat the hydrolyzate and solution B to 75°C, mix, and stir at this temperature for 30 minutes to obtain the product.

[0044] The test results show that the 3d compressive strength of the mortar is 20.2MPa, the 7d compressive strength is 24.9MPa, the 28d compressive strength is 43.2MPa, and the chloride ion diffusion coefficient is 18.4×10 -12 m 2 / s.

[0045] Comparative Example 2

[0046] The cement reinforcing agent, the preparation method comprises the following steps:

[0047] 1) Weigh 35 parts of triethanolamine, 30 parts of diethylene glycol, 10 parts of silica sol, 4 parts of water, 22 parts of ethanol, 3 parts of citric acid, and 0.5 parts of sodium hexametaphosphate by weight.

[0048] 2) Mix water and ethanol evenly to obtain a solution.

[0049] 3) Mix the solution and silica sol to obtain liquid A.

[0050] 4) Mix triethanolamine, diethylene glycol and sodium hexametaphosphate, add citric acid, mix well to obtain liquid B.

[0051] 5) Heat liquid A and liquid B to 75°C, mix, and stir at this temperature for 30 minutes.

[0052] The test results show that the 3d compressive strength of the mortar is 21.5MPa, the 7d compressive strength is 26.1MPa, the 28d compressive strength is 44.3MPa, and the chloride ion diffusion coefficient is 15.6×10 -12 m 2 / s.

[0053] Comparative Example 3

[0054] The cement reinforcing agent, the preparation method comprises the following steps:

[0055] 1) Weigh 35 parts of triethanolamine, 30 parts of diethylene glycol, 8 parts of sodium silicate, 4 parts of silane coupling agent, 4 parts of water, 22 parts of ethanol, 3 parts of citric acid, and 0.5 parts of sodium hexametaphosphate by weight.

[0056] 2) Mix the silane coupling agent, water and ethanol evenly and stir for 4 hours to obtain a hydrolyzate.

[0057] 3) Mix the hydrolyzate and sodium silicate to obtain liquid A.

[0058] 4) Mix triethanolamine, diethylene glycol and sodium hexametaphosphate, add citric acid, mix well to obtain liquid B.

[0059] 5) Heat liquid A and liquid B to 75°C, mix, and stir at this temperature for 30 minutes.

[0060] The test results show that the 3d compressive strength of the mortar is 22.9MPa, the 7d compressive strength is 27.5MPa, the 28d compressive strength is 48.7MPa, and the chloride ion diffusion coefficient is 16.4×10 -12 m 2 / s.

[0061] Comparative Example 4

[0062] The cement reinforcing agent, the preparation method comprises the following steps:

[0063] 1) Weigh 55 parts of triethanolamine, 10 parts of silica sol, 4 parts of silane coupling agent, 4 parts of water, 22 parts of ethanol, 3 parts of citric acid, and 0.5 parts of sodium hexametaphosphate by weight.

[0064] 2) Mix the silane coupling agent, water and ethanol evenly and stir for 4 hours to obtain a hydrolyzate.

[0065] 3) Mix the hydrolyzate and silica sol to obtain liquid A.

[0066] 4) Mix triethanolamine and sodium hexametaphosphate, add citric acid, mix well, and obtain liquid B.

[0067] 5) Heat liquid A and liquid B to 75°C, mix, and stir at this temperature for 30 minutes.

[0068] The test results show that the 3d compressive strength of the mortar is 21.0MPa, the 7d compressive strength is 26.6MPa, the 28d compressive strength is 47.3MPa, and the chloride ion diffusion coefficient is 10.4×10 -12 m 2 / s.

[0069] Comparative Example 5

[0070] The cement reinforcing agent, the preparation method comprises the following steps:

[0071] 1) Weigh 35 parts of calcium formate, 30 parts of diethylene glycol, 8 parts of silica sol, 4 parts of silane coupling agent, 4 parts of water, 22 parts of ethanol, 3 parts of citric acid, and 0.5 parts of sodium hexametaphosphate by weight.

[0072] 2) Mix the silane coupling agent, water and ethanol evenly and stir for 4 hours to obtain a hydrolyzate.

[0073] 3) Mix the hydrolyzate and silica sol to obtain liquid A.

[0074] 4) Mix calcium formate, diethylene glycol and sodium hexametaphosphate, add citric acid, mix well to obtain liquid B.

[0075] 5) Heat liquid A and liquid B to 75°C, mix, and stir at this temperature for 30 minutes.

[0076] The test results show that the 3d compressive strength of the mortar is 22.4MPa, the 7d compressive strength is 27.0MPa, the 28d compressive strength is 48.1MPa, and the chloride ion diffusion coefficient is 16.3×10 -12 m 2 / s.

[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a cement reinforcing agent, characterized in that: The steps include: 1) Weigh 20-40 parts of triethanolamine, 20-40 parts of diethylene glycol, 5-10 parts of silica sol, 3-5 parts of silane coupling agent, 1-5 parts of water, 15-25 parts of ethanol, 1-3 parts of citric acid, and 0.3-1 parts of dispersant by weight. 2) Mix the silane coupling agent, water and ethanol evenly and stir to obtain a hydrolyzate. 3) Mix the hydrolyzate and silica sol to obtain liquid A. 4) Mix triethanolamine, diethylene glycol and dispersant, add citric acid, mix well to obtain liquid B. 5) Heat liquid A and liquid B, mix, and stir while keeping warm to obtain.

2. The method for preparing a cement reinforcing agent according to claim 1, characterized in that: The silica sol is neutral silica sol.

3. The method for preparing a cement reinforcing agent according to claim 1, characterized in that: The silane coupling agent is at least one of KH550, KH560 and KH570.

4. The method for preparing a cement reinforcing agent according to claim 1, characterized in that: The ethanol is anhydrous ethanol.

5. The method for preparing a cement reinforcing agent according to claim 1, characterized in that: The dispersant is at least one of sodium tripolyphosphate, sodium hexametaphosphate and sodium pyrophosphate.

6. The method for preparing a cement reinforcing agent according to claim 1, characterized in that: Step 2) stirring time is 3-5h.

7. The method for preparing a cement reinforcing agent according to claim 1, characterized in that: Step 5) Heat to 70-85°C, keep warm and stir for 30-60 minutes.

8. A cement reinforcing agent, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the cement reinforcing agent according to claim 8 in cement-based building materials.

10. The use according to claim 9, characterized in that: The amount of cement-based reinforcing agent added is 0.3-1% of the mass of the cementitious material.