Ceramic microsphere with amino silane coupling agent fixed on surface and preparation method thereof
By the preparation method of immobilizing aminosilane coupling agent on ceramic microspheres, the problem of difficulty in retaining the activity of the surface group of ceramic microspheres is solved, and the good dispersion and combination of ceramic microspheres in organic and inorganic materials is achieved, which has improved its Modification effect.
Patent Information
- Application Number
- CN202411192619.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
In ceramic materials, the reactive group activity of the surface-fixed silane coupling agent in particular of ceramic microspheres is difficult to retain, which affects its modification effect.
Using a ceramic microsphere preparation method with surface-fixed aminosilane coupling agent, the siloxane is retained by calcined kaolin and amorphous silicon powder slurry configuration, spray drying, sintering, surface modification, alcoholylation and ammonialysis reaction. Reactive activity of groups and amino groups.
Effective deposition of the aminosilane coupling agent fixed on the surface of ceramic microspheres is achieved, the reactive activity of siloxane groups and amino groups is maintained, and the uniform dispersion and binding ability of ceramic microspheres in organic and inorganic materials are improved.
Smart Images

Figure HDA0005015504370000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic microspheres, and particularly relates to ceramic microspheres with an aminosilane coupling agent fixed on the surface thereof and a preparation method thereof. Background Art
[0002] Ceramic microspheres generally refer to inorganic non-metallic sintered bodies with a particle size of micrometers, which are spherical or nearly spherical, and have various forms such as solid, hollow and porous microspheres. They not only have the excellent properties of ceramic materials, but also have the advantages of microsphere particles: 1. Because of its spherical shape, as a reinforcing material for composite materials, it can overcome the anisotropy of irregular-shaped lamellar reinforcing materials such as fibers, needles, spindles, and sheets, reduce the stress concentration generated at the corners, and improve the strength and plasticity of the matrix; 2. Due to the isotropy of ceramic microspheres, under the action of external stress, stress concentration will not be generated on the matrix, so that the castability, plasticity and fluidity of the matrix are greatly improved, which is convenient for the secondary molding of composite materials; 3. Ceramic microspheres can also be used as functional fillers for various conductive media, which can improve the strength, hardness, wear resistance, corrosion resistance, chemical stability and weathering resistance of the matrix; 4. Since the contact form of the microspheres is point contact, the ceramic dispersed phase is added to the matrix in the form of microspheres to avoid the agglomeration of the dispersed phase in the matrix. It is precisely because of these excellent properties that ceramic microspheres are widely used in military industry, medicine, chemical industry, environmental protection, nuclear technology and other fields.
[0003] The surface properties of micron-sized inorganic powder materials such as ceramic microspheres are very different from those of polymer organic systems, which also makes it difficult for inorganic powders to be dispersed well in the material. Therefore, when inorganic powders are added to polymer composite materials, the surface of the inorganic powders must first be modified to make the particle surface organic, improve its lipophilicity and compatibility with the matrix, and enhance the interface bonding ability, so as to exert the function of the inorganic powder. The relevant modification methods can be roughly divided into the following six categories: 1. Surface coverage modification; 2. Chemical coating modification; 3. Precipitation reaction modification; 4. Mechanical chemical reaction; 5. External film layer modification; 6. High-energy surface modification.
[0004] Chemical coating modification is a common modification method that uses chemical reactions to make organic molecules adsorb to the surface of ceramic powders and then coat the ceramic powders, so that the surface of the powder particles has new functions. Hu Xuehui used tartaric acid, EDTA, and sodium D-gluconate as chelating agents to modify barium titanate ceramics in "Preparation and Dielectric Properties of 0-3 Modified Ceramic / Polymer Composite Materials" to study the dielectric properties of modified ceramic materials. Chelating agents can react with metal atoms on the surface of ceramics to form cyclic chelates, among which chelating agents are multidentate ligand complexing agents and are widely used in metallurgy and oilfield descaling. The results show that: first, the effect of interface modification increases with the increase of barium titanate content. When the volume fraction of modified barium titanate is high, the interface modification effect is obvious and the dielectric constant increases more; secondly, the chelate layer acting between the inorganic phase and the organic phase improves the interface connection, which is beneficial to the dispersibility of the inorganic phase, thereby improving the dielectric constant of the system.
[0005] In chemical coating modification, the most commonly used is the surface grafting polymerization coating method, which is to connect the polymer material to the surface of the inorganic particle through chemical reaction. The characteristic of this method is that the polymer modifier that is finally grafted and coated on the modified body is synthesized simultaneously during the modification process. For example, when silicon carbide powder is treated with an organic silicon coupling agent, the organic monomer is grafted on the particle surface through polymerization reaction under suitable conditions to form a polyelectrolyte layer. The dispersion stability of the modified silicon carbide powder in water is much better than that of the unmodified silicon carbide powder.
[0006] The Chinese invention patent application (CN202311256558.1) discloses "A method for modifying ceramic powder, microwave dielectric ceramic slurry, preparation method and application thereof". The application adopts an organic coating method to modify the surface function of ceramic powder, that is, a multifunctional acrylate monomer containing a siloxane group is used, one end of which contains an acrylate group that can participate in the photopolymerization reaction, and the other end contains a siloxane group. The siloxane group can be grafted on the surface of the ceramic powder after hydrolysis, and the acrylate group grafted on the surface of the ceramic powder is exposed, so that the ceramic powder has a photosensitive property. The photosensitive group can undergo a polymerization reaction with the acrylate group in the photosensitive resin used in the ceramic slurry to improve the curing performance of the ceramic slurry.
[0007] The grafting modification of silane coupling agent and ceramic materials depends on the hydroxyl groups on the ceramic surface to form -Si-O- chemical bonds. Wang Xing showed in "Research on the Application of Silane Coupling Agent in Porcelain Repair" that under acidic catalytic conditions, hydrolyzed silane molecules are prone to condensation reactions to form siloxane oligomers, and these siloxane oligomer molecules can continue to condense to form polysiloxane compounds with linear or even network structures. It is generally believed that after the hydrolysis of silane coupling agent, most of the monomers and a small amount of oligomers in the hydrolyzate play a coupling role. If most of the monomer components in the hydrolyzate condense, it is bound to affect the effectiveness of the coupling agent; on the other hand, the hydrolysis reaction of the silane coupling agent introduces organic functional groups on the ceramic powder, which also loses the activity of the siloxane groups on the silane coupling agent.
[0008] In summary, the technical problem to be solved by the present invention is to fix the silane coupling agent on the surface of ceramic materials, especially ceramic microspheres, and retain the reactivity of the two reactive groups on the silane coupling agent, namely the siloxane group (inorganic group) and the amino group (organic group). Summary of the invention
[0009] In order to solve the above technical problems, the present invention provides a ceramic microsphere with an aminosilane coupling agent fixed on the surface.
[0010] Another object of the present invention is to provide a method for preparing ceramic microspheres with aminosilane coupling agents fixed on the surface.
[0011] To achieve the above object, the technical solution adopted by the present invention is: a ceramic microsphere with an aminosilane coupling agent fixed on its surface, the composition and content of which are as follows by mass:
[0012] 45-50 parts of calcined kaolin, 10-25 parts of spherical granular amorphous silicon powder, 45-25 parts of deionized water, 0.3-1.3 parts of dispersant, and 0.3-1.5 parts of binder.
[0013] In a further preferred embodiment, the particle sizes of the calcined kaolin and the spherical amorphous silicon powder are both 30 to 50 nm.
[0014] In a further preferred embodiment, the dispersant is any one of tetramethylammonium hydroxide, sodium hexametaphosphate, polyacrylate, citrate, and sodium humate.
[0015] In a further preferred embodiment, the binder is any one of sodium carboxymethyl cellulose, methyl cellulose, polyvinyl alcohol, polypropylene, saccharin, dextrin, starch and gum arabic.
[0016] In a further preferred embodiment, the first catalyst is any one of a copper-based catalyst and an iron-based catalyst.
[0017] In a further preferred embodiment, the alcoholysis agent is any one of methanol and ethanol.
[0018] In a further preferred embodiment, the second catalyst is hydrated ruthenium trichloride.
[0019] The present invention provides a method for preparing ceramic microspheres with an aminosilane coupling agent fixed on the surface, comprising the following steps:
[0020] The first step is slurry preparation
[0021] 45-50 parts of calcined kaolin with a particle size of 30-50 nm, 10-25 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 45-25 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.3-1.3 parts of a dispersant are added, and after ball milling and mixing for 1.5 hours, 0.3-1.5 parts of a binder are added, and the ball milling and mixing is continued for 2-4 hours to obtain a slurry;
[0022] The second step is spray drying
[0023] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-25000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0024] The third step is microsphere sintering
[0025] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0026] Step 4: Surface modification
[0027] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1 to 2.5 parts of a first catalyst having a particle size of 30 to 50 nm, silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening, the reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours;
[0028] Step 5: Alcoholysis
[0029] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours;
[0030] Step 6: Addition reaction
[0031] The ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and 10 to 25 parts of 3-chloropropylene are subjected to an addition reaction under the action of 1 to 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogen-containing alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0032] Step 7: Ammonolysis
[0033] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor, and subjected to aminolysis reaction with 20 to 50 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85 to 95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5 hours.
[0034] Furthermore, the dispersant is one of tetramethylammonium hydroxide, sodium hexametaphosphate, polyacrylate, citrate, and sodium humate; the binder is one of sodium cellulose, methyl cellulose, polyvinyl alcohol, polypropylene, saccharin, dextrin, starch, and gum arabic; the first catalyst is one of a copper-based catalyst and an iron-based catalyst; the alcoholysis agent is one of methanol and ethanol; and the second catalyst is hydrated ruthenium trichloride.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] The present invention discloses a ceramic microsphere with an aminosilane coupling agent fixed on the surface. The aminosilane coupling agent is fixed on the surface of the ceramic microsphere, and the reactivity of two reactive groups on the silane coupling agent, namely, a siloxane group (inorganic group) and an amino group (organic functional group), is retained. The retained amino group can react with other organic materials, and the retained siloxane group can be combined with other inorganic materials. When used as an additive or filler for coatings or other materials, the aminosilane coupling agent fixed on the surface of the ceramic microsphere can effectively help the ceramic material to be evenly and stably dispersed in an organic system; it can also effectively combine with organic and inorganic substances in the material, so that the ceramic microsphere can effectively form a whole with other materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 These are infrared spectra of ordinary ceramic microspheres (a) and ceramic microspheres with aminosilane coupling agents fixed on their surfaces (b). DETAILED DESCRIPTION
[0038] Example 1
[0039] A method for preparing ceramic microspheres with a particle size of 30 to 50 μm and an aminosilane coupling agent fixed on the surface:
[0040] The first step is slurry preparation
[0041] 45 parts of calcined kaolin with a particle size of 30-50 nm, 10 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 45 parts of deionized water are added to a ball mill, and after ball milling and mixing for 30 minutes, 0.3 parts of dispersant tetramethylammonium hydroxide are added, and after ball milling and mixing for 1.5 hours, 0.3 parts of binder sodium shuttle methyl cellulose are added, and the mixture is ball milled and mixed for 2 hours to obtain a slurry;
[0042] The second step is spray drying
[0043] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 22000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0044] The third step is microsphere sintering
[0045] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0046] Step 4: Surface modification
[0047] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1 part of the first catalyst with a particle size of 30-50 nm, silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening, the reaction temperature is 350-450° C., the reaction pressure is 0.3-0.5 MPa, and the reaction time is 4 hours;
[0048] Step 5: Alcoholysis
[0049] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours;
[0050] Step 6: Addition reaction
[0051] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and an addition reaction is carried out with 10 parts of 3-chloropropylene in the presence of 1 part of a second catalyst with a particle size of 30 to 50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0052] Step 7: Ammonolysis
[0053] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 20 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0054] Example 2
[0055] A method for preparing ceramic microspheres with a particle size of 50 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0056] The first step is slurry preparation
[0057] 46 parts of calcined kaolin with a particle size of 30-50 nm, 12 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 42 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.4 parts of dispersant sodium hexametaphosphate are added, and after ball milling and mixing for 1.5 hours, 0.4 parts of binder methyl cellulose are added, and the mixture is ball milled and mixed for 2.5 hours to obtain a slurry;
[0058] The second step is spray drying
[0059] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 15000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0060] The third step is microsphere sintering
[0061] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0062] Step 4: Surface modification
[0063] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.5 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0064] Step 5: Alcoholysis
[0065] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 35 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0066] Step 6: Addition reaction
[0067] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 15 parts of 3-chloropropylene in the presence of 1.5 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0068] Step 7: Ammonolysis
[0069] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 25 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0070] Example 3
[0071] A method for preparing ceramic microspheres with a particle size of 80 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0072] The first step is slurry preparation
[0073] 47 parts of calcined kaolin with a particle size of 30-50 nm, 14 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 40 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.5 parts of dispersant polyacrylate are added, and after ball milling and mixing for 1.5 hours, 0.5 parts of binder gum arabic are added, and the mixture is ball milled and mixed for 2 hours to obtain a slurry;
[0074] The second step is spray drying
[0075] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0076] The third step is microsphere sintering
[0077] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0078] Step 4: Surface modification
[0079] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.7 parts of a first catalyst having a particle size of 30 to 50 nm. The silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0080] Step 5: Alcoholysis
[0081] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 32 parts of an alcoholysis agent under the protection of an inert gas, and the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, which is filtered to obtain ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface, the reaction temperature is 60-70° C., and the reaction time is 4 hours;
[0082] Step 6: Addition reaction
[0083] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 13 parts of 3-chloropropylene in the presence of 1.8 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0084] Step 7: Ammonolysis
[0085] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 23 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0086] Example 4
[0087] A method for preparing ceramic microspheres with a particle size of 30 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0088] The first step is slurry preparation
[0089] 48 parts of calcined kaolin with a particle size of 30-50 nm, 16 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 38 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.6 parts of dispersant citrate are added, and after ball milling and mixing for 1.5 hours, 0.6 parts of binder dextrin are added, and the ball milling and mixing is continued for 2.5 hours to obtain a slurry;
[0090] The second step is spray drying
[0091] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-20000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0092] The third step is microsphere sintering
[0093] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0094] Step 4: Surface modification
[0095] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.3 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0096] Step 5: Alcoholysis
[0097] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 35 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0098] Step 6: Addition reaction
[0099] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 18 parts of 3-chloropropylene in the presence of 1.6 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0100] Step 7: Ammonolysis
[0101] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 30 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0102] Example 5
[0103] A method for preparing ceramic microspheres with a particle size of 50 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0104] The first step is slurry preparation
[0105] 49 parts of calcined kaolin with a particle size of 30-50 nm, 18 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 36 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.7 parts of dispersant sodium humate are added, and after ball milling and mixing for 1.5 hours, 0.8 parts of binder starch are added, and the mixture is ball milled and mixed for 2.5 hours to obtain a slurry;
[0106] The second step is spray drying
[0107] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-12000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0108] The third step is microsphere sintering
[0109] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0110] Step 4: Surface modification
[0111] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2 parts of a first catalyst having a particle size of 30 to 50 nm. The silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0112] Step 5: Alcoholysis
[0113] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 50 parts of an alcoholysis agent under the protection of an inert gas, and the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, which is filtered to obtain ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface, the reaction temperature is 60-70° C., and the reaction time is 4 hours;
[0114] Step 6: Addition reaction
[0115] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and 10 to 25 parts of 3-chloropropylene are subjected to an addition reaction under the action of 1.7 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0116] Step 7: Ammonolysis
[0117] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 45 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0118] Example 6
[0119] A method for preparing ceramic microspheres with a particle size of 30 to 50 μm and an aminosilane coupling agent fixed on the surface:
[0120] The first step is slurry preparation
[0121] 50 parts of calcined kaolin with a particle size of 30-50 nm, 19 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 34 parts of deionized water are added into a ball mill, and after ball milling the mixture for 30 minutes, 0.8 parts of dispersant sodium humate are added, and after ball milling the mixture for 1.5 hours, 1.0 parts of binder polyvinyl alcohol are added, and the mixture is ball milled for 2.5 hours to obtain a slurry;
[0122] The second step is spray drying
[0123] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 25000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0124] The third step is microsphere sintering
[0125] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0126] Step 4: Surface modification
[0127] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.3 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0128] Step 5: Alcoholysis
[0129] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 55 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0130] Step 6: Addition reaction
[0131] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and subjected to an addition reaction with 20 parts of 3-chloropropylene under the action of 2.4 parts of a second catalyst with a particle size of 30-50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70-80° C., and the reaction time is 4 hours;
[0132] Step 7: Ammonolysis
[0133] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 28 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0134] Example 7
[0135] A method for preparing ceramic microspheres with a particle size of 50 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0136] The first step is slurry preparation
[0137] 49 parts of calcined kaolin with a particle size of 30-50 nm, 20 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 32 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.9 parts of dispersant citrate are added, and after ball milling and mixing for 1.5 hours, 1.2 parts of binder polypropylene are added, and the mixture is ball milled and mixed for 3 hours to obtain a slurry;
[0138] The second step is spray drying
[0139] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 17000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0140] The third step is microsphere sintering
[0141] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0142] Step 4: Surface modification
[0143] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.5 parts of a first catalyst having a particle size of 30 to 50 nm. The silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0144] Step 5: Alcoholysis
[0145] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 65 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0146] Step 6: Addition reaction
[0147] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 19 parts of 3-chloropropylene in the presence of 2.3 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0148] Step 7: Ammonolysis
[0149] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 48 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0150] Example 8
[0151] A method for preparing ceramic microspheres with a particle size of 80 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0152] The first step is slurry preparation
[0153] 48 parts of calcined kaolin with a particle size of 30-50 nm, 22 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 30 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 1.0 part of a dispersant polyacrylate is added, and after ball milling and mixing for 1.5 hours, 1.3 parts of a binder dextrin is added, and the ball milling and mixing is continued for 3 hours to obtain a slurry;
[0154] The second step is spray drying
[0155] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 9000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0156] The third step is microsphere sintering
[0157] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0158] Step 4: Surface modification
[0159] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.1 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0160] Step 5: Alcoholysis
[0161] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 65 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0162] Step 6: Addition reaction
[0163] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and subjected to addition reaction with 20 parts of 3-chloropropylene under the action of 1.4 parts of a second catalyst with a particle size of 30-50 nm, the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70-80° C., and the reaction time is 4 hours;
[0164] Step 7: Ammonolysis
[0165] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor, and subjected to an aminolysis reaction with 19 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0166] Example 9
[0167] A method for preparing ceramic microspheres with a particle size of 30 to 80 μm and an aminosilane coupling agent fixed on the surface:
[0168] The first step is slurry preparation
[0169] 47 parts of calcined kaolin with a particle size of 30 to 50 nm, 24 parts of spherical amorphous silicon powder with a particle size of 30 to 50 nm, and 28 parts of deionized water are added to a ball mill, and after ball milling and mixing for 30 minutes, 1.1 parts of dispersant sodium hexametaphosphate are added, and after ball milling and mixing for 1.5 hours, 1.4 parts of binder sodium carboxymethyl cellulose are added, and the mixture is ball milled and mixed for 3.5 hours to obtain a slurry;
[0170] The second step is spray drying
[0171] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 21000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0172] The third step is microsphere sintering
[0173] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0174] Step 4: Surface modification
[0175] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 2.3 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0176] Step 5: Alcoholysis
[0177] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 70 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are obtained by filtration, and the reaction temperature is 60-70° C. and the reaction time is 4 hours;
[0178] Step 6: Addition reaction
[0179] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and are subjected to an addition reaction with 17 parts of 3-chloropropylene in the presence of 2.0 parts of a second catalyst having a particle size of 30 to 50 nm, wherein the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0180] Step 7: Ammonolysis
[0181] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to an aminolysis reaction with 53 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate an aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with the aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0182] Example 10
[0183] A method for preparing ceramic microspheres with a particle size of 50 to 100 μm and an aminosilane coupling agent fixed on the surface:
[0184] The first step is slurry preparation
[0185] 46 parts of calcined kaolin with a particle size of 30-50 nm, 25 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 25 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 1.3 parts of dispersant tetramethylammonium hydroxide are added, and after ball milling and mixing for 1.5 hours, 1.5 parts of binder methyl cellulose are added, and the mixture is ball milled and mixed for another 4 hours to obtain a slurry;
[0186] The second step is spray drying
[0187] The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 13000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min;
[0188] The third step is microsphere sintering
[0189] The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres;
[0190] Step 4: Surface modification
[0191] The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1.6 parts of a first catalyst having a particle size of 30 to 50 nm. Silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening. The reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours.
[0192] Step 5: Alcoholysis
[0193] The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 45 parts of an alcoholysis agent under the protection of an inert gas, and the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, which is filtered to obtain ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface, the reaction temperature is 60-70° C., and the reaction time is 4 hours;
[0194] Step 6: Addition reaction
[0195] The ceramic microspheres with hydrogenated alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and an addition reaction is carried out with 18 parts of 3-chloropropylene in the presence of 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogenated alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropylalkoxysilane, and the ceramic microspheres with 3-chloropropylalkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours;
[0196] Step 7: Ammonolysis
[0197] The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor and subjected to aminolysis reaction with 45 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85-95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5h.
[0198] Figure 1 In the figure, a is the infrared spectrum of ceramic microspheres with aminosilane coupling agent fixed on the surface, and b is the infrared spectrum of ordinary ceramic microspheres. Both a and b have obvious absorption peaks near 3400-1, 1192cm-1 and 1084cm-1. The absorption peak near 3400-1 is the stretching vibration peak of -OH, and the absorption peaks near 1192cm-1 and 1084cm-1 are the stretching vibration peaks of Si-O. In comparison, 3349cm-1 in a is the stretching vibration peak of N-H, and 2939cm-1 is the saturated carbon-hydrogen bond. The stretching vibration absorption peak of 1365cm-1 is the stretching vibration of C—N, indicating that the ceramic microspheres with aminosilane coupling agent fixed on the surface have molecular bonds of organic groups, while the peak areas of the absorption peaks near 1192cm-1 and 1084cm-1 in Figure a are significantly larger than those in Figure b, indicating that the ceramic microspheres with aminosilane coupling agent fixed on the surface have more inorganic groups, which indirectly reflects the coexistence of inorganic and organic groups in the ceramic microspheres, which proves that the present application successfully fixed the aminosilane coupling agent on the surface of the ceramic microspheres.
Claims
1. A ceramic microsphere with an aminosilane coupling agent fixed on its surface, characterized in that: Its composition and content by mass are: 45-50 parts of calcined kaolin, 10-25 parts of spherical granular amorphous silicon powder, 45-25 parts of deionized water, 0.3-1.3 parts of dispersant, 0.3-1.5 parts of binder, and 30-75 parts of alcoholysis agent.
2. The ceramic microspheres with aminosilane coupling agent fixed on the surface according to claim 1, characterized in that: The particle sizes of the calcined kaolin and spherical amorphous silicon powder are both 30-50nm.
3. The ceramic microspheres with aminosilane coupling agent fixed on the surface according to claim 1, characterized in that: The dispersant is any one of tetramethylammonium hydroxide, sodium hexametaphosphate, polyacrylate, citrate and sodium humate.
4. The ceramic microspheres with aminosilane coupling agent fixed on the surface according to claim 1, characterized in that: The binder is any one of sodium cellulose, methyl cellulose, polyvinyl alcohol, polypropylene, saccharin, dextrin, starch and gum arabic.
5. The ceramic microspheres with aminosilane coupling agent fixed on the surface according to claim 1, characterized in that: The first catalyst is any one of a copper-based catalyst and an iron-based catalyst.
6. The ceramic microspheres with aminosilane coupling agent fixed on the surface according to claim 1, characterized in that: The alcoholysis agent is any one of methanol and ethanol.
7. The ceramic microspheres with aminosilane coupling agent fixed on the surface according to claim 1, characterized in that: The second catalyst is hydrated ruthenium trichloride.
8. A method for preparing ceramic microspheres with aminosilane coupling agents fixed on the surface as claimed in any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: The first step is slurry preparation 45-50 parts of calcined kaolin with a particle size of 30-50 nm, 10-25 parts of spherical amorphous silicon powder with a particle size of 30-50 nm, and 45-25 parts of deionized water are added into a ball mill, and after ball milling and mixing for 30 minutes, 0.3-1.3 parts of a dispersant are added, and after ball milling and mixing for 1.5 hours, 0.3-1.5 parts of a binder are added, and the ball milling and mixing is continued for 2-4 hours to obtain a slurry; The second step is spray drying The slurry obtained in the first step is granulated and dried by a centrifugal spray dryer to obtain kaolin microspheres. The hot air inlet temperature of the centrifugal spray dryer is 200-250°C, the outlet temperature is 80-90°C, the centrifugal atomization speed is 8000-25000r / min, the slurry atomization pressure is 0.08-0.1MPa, and the feed rate is 100mL / min; The third step is microsphere sintering The kaolin microspheres obtained in the second step were first heated to 900°C under argon protection, then cooled to room temperature, then heated to 1200°C and kept for 1 hour, then cooled to room temperature, then heated to 1400°C and kept for 4 hours, and then cooled to room temperature to obtain ceramic microspheres; Step 4: Surface modification The ceramic microspheres obtained in the third step are added into a fluidized bed reactor, and reacted with gaseous hydrogen chloride under the action of 1 to 2.5 parts of a first catalyst having a particle size of 30 to 50 nm, silicon on the surface of the ceramic microspheres reacts with hydrogen chloride to generate trichlorosilane, and the ceramic microspheres with trichlorosilane fixed on the surface are obtained by screening, the reaction temperature is 350 to 450° C., the reaction pressure is 0.3 to 0.5 MPa, and the reaction time is 4 hours; Step 5: Alcoholysis The ceramic microspheres with trichlorosilane fixed on the surface obtained in the fourth step are added into a reactor with a condensation reflux device, and are subjected to alcoholysis reaction with 30 to 75 parts of an alcoholysis agent under the protection of an inert gas, wherein the trichlorosilane on the surface of the ceramic microspheres reacts with the alcoholysis agent to generate hydrogen-containing alkoxysilane, and the ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface are filtered to obtain the ceramic microspheres, the reaction temperature is 60 to 70° C., and the reaction time is 4 hours; Step 6: Addition reaction The ceramic microspheres with hydrogen-containing alkoxysilane fixed on the surface obtained in the fifth step are added into a reactor with a condensation reflux device, and 10 to 25 parts of 3-chloropropylene are subjected to an addition reaction under the action of 1 to 2.5 parts of a second catalyst with a particle size of 30 to 50 nm, and the hydrogen-containing alkoxysilane on the surface of the ceramic microspheres reacts with 3-chloropropylene to generate 3-chloropropyl alkoxysilane, and the ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface are obtained by screening, the reaction temperature is 70 to 80° C., and the reaction time is 4 hours; Step 7: Ammonolysis The ceramic microspheres with 3-chloropropyl alkoxysilane fixed on the surface obtained in the sixth step are added into the reactor, and subjected to aminolysis reaction with 20 to 50 parts of ethylenediamine. The 3-chloropropyl alkoxysilane on the surface of the ceramic microspheres reacts with ethylenediamine to generate aminosilane coupling agent. The reaction temperature is 85 to 95°C. After the reaction is completed, the ceramic microspheres with aminosilane coupling agent fixed on the surface are filtered to obtain the ceramic microspheres. The reaction time is 5 hours.
9. The method for preparing ceramic microspheres with aminosilane coupling agents fixed on the surface according to claim 8, characterized in that: The ceramic microspheres with aminosilane coupling agents fixed on the surface have a particle size of 30 to 100 μm and the aminosilane coupling agents are fixed on the surface.