Rapidly-dried SiC honeycomb ceramic skin, SiC honeycomb ceramic with skin and preparation method of honeycomb ceramic

SiC was solved by using a specific proportion of silicon carbide powder, metal silicon powder, ceramic fibers, cellulose, silicon sol and surfactant in SiC honeycomb ceramic skin, and using mixing and vacuum treatment of mud training machines. The problem of the long drying time of honeycomb ceramic skin achieves rapid drying and efficient production.

CN119080532AInactive Publication Date: 2024-12-06YIXING PRINCE CERAMICS

Patent Information

Application Number
CN202411152323.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The drying time of existing SiC honeycomb ceramic skins usually exceeds 24 hours, resulting in low turnover efficiency of the dryer.

Method used

50 to 90 parts of silicon carbide powder, 5 to 15 parts of metal silicon powder, 3 to 10% ceramic fiber, 0.5 to 1.5% cellulose, 20 to 40% silicon sol, 0.3 to 1.0% defoaming agent is used. The combination of 0.3-1.0% surfactant potassium laurate is achieved by dry mixing and wet mixing process of the mud training machine and vacuum treatment to achieve rapid drying.

Benefits of technology

Under the drying conditions of 40-70°C, the honeycomb ceramic skin can be dried within 2.0-4 hours without causing skin opening, which significantly improves the turnover efficiency of the drying room.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a rapidly-dried SiC honeycomb ceramic sheath, SiC honeycomb ceramic with the sheath and a preparation method of the honeycomb ceramic, the sheath comprises the following raw materials in parts by weight: 50-90 parts of silicon carbide powder, the silicon carbide powder comprises 45-55 parts of coarse-grained silicon carbide, 15-23 parts of medium-grained silicon carbide, 10-17 parts of fine-grained silicon carbide and 5-15 parts of metal silicon powder, and the average particle size of the silicon carbide powder is 3-7 [mu] m; the outer skin further comprises ceramic fibers accounting for 3-10% of the sum of the weight of the silicon carbide powder and the weight of the metal silicon powder, cellulose accounting for 0.5-1.5% of the sum of the weight of the silicon carbide powder and the weight of the metal silicon powder, silica sol accounting for 20-40% of the sum of the weight of the silicon carbide powder and the weight of the metal silicon powder, an antifoaming agent accounting for 0.3-1.0% of the sum of the weight of the metal silicon powder and the sum of the weight of the silicon carbide powder and the weight of the metal silicon powder. The preparation method has the beneficial effects that the dispersity and compactness of the pug are greatly improved, the pug can be quickly dried at 40-70 DEG C after being coated with an outer skin, the drying time is less than 4 hours, and the skin cannot be opened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of honeycomb ceramics, and in particular to a rapidly dried SiC honeycomb ceramic skin, a SiC honeycomb ceramic having the skin, and a method for preparing the honeycomb ceramic. Background Art

[0002] At present, the honeycomb ceramic materials widely used in the field of motor vehicle exhaust purification are mainly cordierite and silicon carbide. Although the former cordierite has low production cost and small thermal expansion coefficient, it has low strength, low thermal conductivity and poor heat resistance, which limits its scope of use and life in engine exhaust purification. Silicon carbide honeycomb ceramics have high strength and high thermal conductivity, good reliability and durability under high temperature conditions, and have become the preferred material for renewable particulate filters; but its thermal expansion coefficient is high, and it cannot be completed in large-scale one-piece molding. The industry generally generates small rectangular blocks of 40*40mm first, then cuts them into the required diameter after splicing, and then coats them with a layer of high-temperature resistant outer skin.

[0003] As a composite material, the main purpose of the skin slurry is to protect the blank, so that it will not be damaged during transportation and use, especially in the use environment of rapid cooling and heating, the blank will not crack due to stress caused by the large temperature difference between the inside and outside. Therefore, after the skin slurry is cured, it is necessary to have better heat shock resistance and skin strength, and its thermal expansion coefficient and thermal conductivity should be close to those of the silicon carbide blank and silicon carbide splicing slurry. Further preferably, the thermal expansion coefficient of the skin slurry is slightly smaller than that of the main material, and while the expansion and contraction are basically the same, it can alleviate the volume expansion caused by the heat of the main material. At the same time, the thermal conductivity of the skin needs to be close to that of the silicon carbide blank to prevent the temperature difference between the inside and outside from being too large due to the difference in thermal conductivity, resulting in stress and cracking.

[0004] There are many kinds of outer skin structure ratios for cordierite-based honeycomb ceramics. CN116903394A discloses a multi-grade SiO2 aggregate ratio that enhances thermal shock resistance, acid resistance, and high temperature resistance after acid soaking; CN112608627A discloses a cordierite peripheral coating material with low thermal expansion coefficient, high strength, and high thermal shock resistance prepared from multi-grade silicon ball powder; CN103480433A, CN115536375A, and CN103044031A are all peripheral coatings prepared with cordierite powder or cordierite component structure chemical ratios. Although such inventions obtain an outer skin structure that is resistant to high thermal shock, their drying time is >24h, even up to 48h, which reduces the turnover efficiency of the drying room. Summary of the invention

[0005] Purpose of the invention:

[0006] In order to overcome the problems existing in the prior art, the present invention provides a quickly dried SiC honeycomb ceramic skin, a SiC honeycomb ceramic having the skin and a method for preparing the honeycomb ceramic, which solves the problem that although the skin structure of the SiC honeycomb ceramic in the prior art can withstand high thermal shock, its drying time is greater than 24 hours, even reaching 48 hours, which reduces the turnover efficiency of the drying room.

[0007] In order to solve the above problems, the present invention adopts the following technical solutions:

[0008] A fast-drying SiC honeycomb ceramic skin, wherein the raw materials of the skin include 50 to 90 parts by weight of silicon carbide powder, of which coarse-grained silicon carbide accounts for 45 to 55 parts with an average particle size of 95 to 105 μm, medium-grained silicon carbide accounts for 15 to 23 parts with an average particle size of 25 to 35 μm, fine-grained silicon carbide accounts for 10 to 17 parts with an average particle size of 3 to 7 μm; and 5 to 15 parts of metallic silicon powder with an average particle size of 3 to 7 μm.

[0009] The outer skin also includes 3-10% of ceramic fiber, 0.5-1.5% of cellulose, 20-40% of silica sol, 0.3-1.0% of defoaming agent, 0.3-1.0% of surfactant potassium laurate, and 15-25% of water, accounting for the total weight of silicon carbide powder and metal silicon powder.

[0010] Preferably, the sum of the parts of silicon carbide powder and the parts of metallic silicon powder is 100 parts.

[0011] Preferably, the raw materials of the outer skin include 55 parts of coarse-grained silicon carbide, 20 parts of medium-grained silicon carbide, 10 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 8% of ceramic fiber, 1.2% of cellulose, 30% of silica sol, 0.3% of defoaming agent, and 0.8% of surfactant potassium laurate, which accounts for the total weight of silicon carbide powder and metallic silicon powder.

[0012] Preferably, the raw materials of the outer skin include 53 parts of coarse-grained silicon carbide, 15 parts of medium-grained silicon carbide, 17 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 5% of ceramic fiber, 0.8% of cellulose, 25% of silica sol, 0.8% of defoaming agent, and 0.8% of surfactant potassium laurate, which accounts for the total weight of silicon carbide powder and metallic silicon powder.

[0013] Preferably, the model of the defoaming agent is GPE3000.

[0014] The invention also discloses a SiC honeycomb ceramic, comprising a honeycomb ceramic body and a skin of the structure above coated on the surface of the honeycomb ceramic body.

[0015] Preferably, the honeycomb ceramic body comprises, by weight, 70 to 85 parts of silicon carbide, 15 to 25 parts of metallic silicon, 0.5 to 2 parts of strontium carbonate, 0.5 to 2 parts of aluminum oxide and 0.5 to 3 parts of clay.

[0016] The preparation method of the SiC honeycomb ceramic comprises the following steps:

[0017] S1. Pour coarse, medium and fine silicon carbide powders and fibers into a mud kneading machine and dry mix them at a rotation speed of 50 Hz for 5 to 15 minutes to obtain a mixed powder;

[0018] S2. Pour silica sol, water, potassium laurate and GPE3000 into a mixing barrel and stir for 3 minutes, then pour into a mud kneading machine, wet mix at a rotation frequency of 50 Hz, rotate forward for 5 to 10 minutes, and reverse for 5 to 10 minutes. During this period, maintain the vacuum degree at -0.8 to -1.0 MPa to obtain an outer skin coating material.

[0019] S3, applying the outer skin coating material obtained in step S2 to the periphery of the honeycomb ceramic body, and then putting it into a drying room at 40-70° C. for rapid drying for 2.0-4 hours to obtain a silicon carbide honeycomb ceramic body.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following advantages: by adding a small amount of surfactant and defoaming agent, and using a mud kneading machine to wet mix the coating material under vacuum, the dispersion and density of the mud material can be greatly improved, so that the mud can be quickly dried at 40-70°C after coating, and the drying time is less than 4h without peeling. DETAILED DESCRIPTION

[0021] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.

[0022] Any feature disclosed in this specification (including any additional claims and abstract), unless otherwise stated, may be replaced by other alternative features that are equivalent or have similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.

[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below.

[0024] A fast-drying SiC honeycomb ceramic skin, wherein the raw materials of the skin include 50 to 90 parts by weight of silicon carbide powder, of which coarse-grained silicon carbide accounts for 45 to 55 parts with an average particle size of 95 to 105 μm, medium-grained silicon carbide accounts for 15 to 23 parts with an average particle size of 25 to 35 μm, fine-grained silicon carbide accounts for 10 to 17 parts with an average particle size of 3 to 7 μm; and 5 to 15 parts of metallic silicon powder with an average particle size of 3 to 7 μm.

[0025] The outer skin also includes 3-10% of ceramic fiber, 0.5-1.5% of cellulose, 20-40% of silica sol, 0.3-1.0% of defoaming agent, 0.3-1.0% of surfactant potassium laurate, and 15-25% of water, accounting for the total weight of silicon carbide powder and metal silicon powder.

[0026] Preferably, the sum of the parts of silicon carbide powder and the parts of metallic silicon powder is 100 parts.

[0027] Preferably, the raw materials of the outer skin include 55 parts of coarse-grained silicon carbide, 20 parts of medium-grained silicon carbide, 10 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 8% of ceramic fiber, 1.2% of cellulose, 30% of silica sol, 0.3% of defoaming agent, and 0.8% of surfactant potassium laurate, which accounts for the total weight of silicon carbide powder and metallic silicon powder.

[0028] Preferably, the raw materials of the outer skin include 53 parts of coarse-grained silicon carbide, 15 parts of medium-grained silicon carbide, 17 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 5% of ceramic fiber, 0.8% of cellulose, 25% of silica sol, 0.8% of defoaming agent, and 0.8% of surfactant potassium laurate, which accounts for the total weight of silicon carbide powder and metallic silicon powder.

[0029] Preferably, the model of the defoaming agent is GPE3000.

[0030] The three-level grading is carried out using coarse particles of 95-105μm, medium particles of 25-35μm, and fine particles of 3-7μm. The density of the mud is improved by adding 0.3-1.0% of the defoaming agent GPE3000 and vacuuming the mixing process.

[0031] By adding 0.3-1.0% potassium laurate as a surfactant, the agglomeration caused by excessively fine powder during the mixing process is reduced. At the same time, the mud kneading machine is made to mix the materials in forward and reverse rotations to improve the uniformity of the mud, so that the mud shrinks uniformly during the rapid drying process without generating cracks.

[0032] The invention also discloses a SiC honeycomb ceramic, comprising a honeycomb ceramic body and a skin of the structure above coated on the surface of the honeycomb ceramic body.

[0033] Preferably, the honeycomb ceramic body comprises, by weight, 70 to 85 parts of silicon carbide, 15 to 25 parts of metallic silicon, 0.5 to 2 parts of strontium carbonate, 0.5 to 2 parts of aluminum oxide and 0.5 to 3 parts of clay.

[0034] The preparation method of the SiC honeycomb ceramic comprises the following steps:

[0035] S1. Pour coarse, medium and fine silicon carbide powders and fibers into a mud kneading machine and dry mix them at a rotation speed of 50 Hz for 5 to 15 minutes to obtain a mixed powder;

[0036] S2. Pour silica sol, water, potassium laurate and GPE3000 into a mixing barrel and stir for 3 minutes, then pour into a mud kneading machine, wet mix at a rotation frequency of 50 Hz, rotate forward for 5 to 10 minutes, and reverse for 5 to 10 minutes. During this period, maintain the vacuum degree at -0.8 to -1.0 MPa to obtain an outer skin coating material.

[0037] S3, applying the outer skin coating material obtained in step S2 to the periphery of the honeycomb ceramic body, and then putting it into a drying room at 40-70° C. for rapid drying for 2.0-4 hours to obtain a silicon carbide honeycomb ceramic body.

[0038] Step S1 and step S2 are methods for preparing the SiC honeycomb ceramic skin, and step S3 is a method for coating the skin coating material onto the honeycomb ceramic body.

[0039] Embodiment 1:

[0040] The above-mentioned SiC honeycomb ceramic preparation method is adopted, and the raw materials of the outer skin include 45 parts of coarse-grained silicon carbide, 23 parts of medium-grained silicon carbide, 17 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 3% of ceramic fiber, 0.5% of cellulose, 20% of silica sol, 1% of defoaming agent, and 1% of surfactant potassium laurate, which accounts for the total weight of silicon carbide powder and metallic silicon powder.

[0041] Embodiment 2:

[0042] The above-mentioned SiC honeycomb ceramic preparation method is adopted, and the raw materials of the outer skin include 55 parts of coarse-grained silicon carbide, 23 parts of medium-grained silicon carbide, 17 parts of fine-grained silicon carbide, and 5 parts of metallic silicon powder; it also includes 10% of ceramic fiber accounting for the sum of the weight of silicon carbide powder and metallic silicon powder, 0.8% of cellulose, 25% of silica sol, 0.5% of defoaming agent, and 0.5% of surfactant potassium laurate.

[0043] Embodiment 3:

[0044] The above-mentioned SiC honeycomb ceramic preparation method is adopted, and the raw materials of the outer skin include 55 parts of coarse-grained silicon carbide, 20 parts of medium-grained silicon carbide, 10 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 8% of ceramic fiber, 1.2% of cellulose, 30% of silica sol, 0.3% of defoaming agent, and 0.8% of surfactant potassium laurate.

[0045] Embodiment 4:

[0046] The above-mentioned SiC honeycomb ceramic preparation method is adopted, and the raw materials of the outer skin include 53 parts of coarse-grained silicon carbide, 15 parts of medium-grained silicon carbide, 17 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; it also includes 5% of ceramic fiber, which accounts for 0.8% of cellulose, 25% of silica sol, 0.8% of defoaming agent, and 0.8% of surfactant potassium laurate.

[0047] Embodiment 5:

[0048] The above-mentioned SiC honeycomb ceramic preparation method is adopted, and the raw materials of the outer skin include 55 parts of coarse-grained silicon carbide, 23 parts of medium-grained silicon carbide, 10 parts of fine-grained silicon carbide, and 12 parts of metallic silicon powder; it also includes 10% of ceramic fiber accounting for the sum of the weight of silicon carbide powder and metallic silicon powder, 1.5% of cellulose, 40% of silica sol, 0.3% of defoaming agent, and 0.8% of surfactant potassium laurate.

[0049] The differences between Examples 1-5 are shown in the following table:

[0050]

[0051]

[0052] The honeycomb ceramic structures provided by the above five embodiments were subjected to performance tests, including drying time, thermal shock resistance, and skin strength and powder loss tests. The specific test contents are as follows:

[0053] S1. Drying time test of the outer skin: put the product into a drying room at 40-70℃, weigh the product, and determine that the drying is complete when the product weight no longer decreases. This time is the drying time. At the same time, pay attention to the outer skin not cracking. If the skin cracks, the drying temperature and time will be invalid;

[0054] S2. Thermal shock test: Place the dried silicon carbide honeycomb ceramic structure into a muffle furnace that has reached the set temperature, keep it warm for 30 minutes, then take it out and observe whether the outer skin is cracked or whether there is a cracking sound. If it is not cracked, cool the product to room temperature and place it back into the muffle furnace and repeat the above process twice. If the three thermal shock tests are qualified, increase the temperature by 50°C and repeat the above process again until the product cracks. The initial thermal shock temperature is set to 400°C;

[0055] S3. Powder loss test: The dried silicon carbide honeycomb ceramic structure is placed in a muffle furnace at 600°C for 30 minutes, then taken out and cooled to room temperature. The outer skin is then scraped horizontally with an iron sheet, and the scraped powder is weighed.

[0056] The test structures of the five embodiments are as follows:

[0057]

[0058] Through experiments and verification, it is shown that the outer skin structures of the above embodiments can be dried within 4 hours after coating without peeling, and the effects of Embodiments 3 and 4 are better.

[0059] The purpose of the above embodiments is to exemplarily reproduce and deduce the technical solution of the present invention, and to fully describe the technical solution, purpose and effect of the present invention. Its purpose is to make the public understand the disclosed content of the present invention more thoroughly and comprehensively, and it does not limit the scope of protection of the present invention.

[0060] The above embodiments are not exhaustive enumerations of the present invention, and there may be multiple other implementations not listed. Any replacement and improvement made without violating the concept of the present invention shall fall within the protection scope of the present invention.

Claims

1. A fast-drying SiC honeycomb ceramic skin, characterized in that: The raw materials of the outer shell include 50 to 90 parts by weight of silicon carbide powder, of which coarse-grained silicon carbide accounts for 45 to 55 parts with an average particle size of 95 to 105 μm, medium-grained silicon carbide accounts for 15 to 23 parts with an average particle size of 25 to 35 μm, fine-grained silicon carbide accounts for 10 to 17 parts with an average particle size of 3 to 7 μm; and 5 to 15 parts of metallic silicon powder with an average particle size of 3 to 7 μm. The outer skin also includes 3-10% of ceramic fiber, 0.5-1.5% of cellulose, 20-40% of silica sol, 0.3-1.0% of defoaming agent, 0.3-1.0% of surfactant potassium laurate, and 15-25% of water, accounting for the total weight of silicon carbide powder and metallic silicon powder.

2. The fast-drying SiC honeycomb ceramic skin according to claim 1, characterized in that: The total of the parts of silicon carbide powder and the parts of metallic silicon powder is 100 parts.

3. The fast-drying SiC honeycomb ceramic skin according to claim 1, characterized in that: The raw materials of the outer skin include 55 parts of coarse-grained silicon carbide, 20 parts of medium-grained silicon carbide, 10 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; and also include 8% of the total weight of the silicon carbide powder and the metallic silicon powder, ceramic fiber, 1.2% of cellulose, 30% of silica sol, 0.3% of a defoaming agent, and 0.8% of a surfactant, potassium laurate.

4. The fast-drying SiC honeycomb ceramic skin according to claim 1, characterized in that: The raw materials of the outer skin include 53 parts of coarse-grained silicon carbide, 15 parts of medium-grained silicon carbide, 17 parts of fine-grained silicon carbide, and 15 parts of metallic silicon powder; and also include 5% of ceramic fiber, 0.8% of cellulose, 25% of silica sol, 0.8% of defoaming agent, and 0.8% of surfactant potassium laurate, which accounts for 5% of the total weight of the silicon carbide powder and the metallic silicon powder.

5. The fast-drying SiC honeycomb ceramic skin according to claim 1, characterized in that: The model of the defoamer is GPE3000.

6. A SiC honeycomb ceramic, characterized in that: The invention comprises a honeycomb ceramic body and a skin coated on the surface of the honeycomb ceramic body as claimed in any one of claims 1 to 5.

7. The SiC honeycomb ceramic according to claim 6, characterized in that: The honeycomb ceramic body comprises 70 to 85 parts of silicon carbide, 15 to 25 parts of metallic silicon, 0.5 to 2 parts of strontium carbonate, 0.5 to 2 parts of aluminum oxide and 0.5 to 3 parts of clay in parts by weight.

8. A method for preparing a SiC honeycomb ceramic according to claim 6 or 7, characterized in that: The following steps are involved: S1. Pour coarse, medium and fine silicon carbide powders and fibers into a mud kneader and dry mix them at a speed of 50 Hz for 5 to 15 minutes to obtain a mixed powder; S2. Pour silica sol, water, potassium laurate and GPE3000 into a mixing barrel and stir for 3 minutes, then pour into a mud kneader and wet mix at a rotation speed of 50 Hz, rotate forward for 5 to 10 minutes and reverse for 5 to 10 minutes, during which the vacuum degree is maintained at -0.8 to -1.0 MPa to obtain an outer coating material. S3. Apply the outer skin coating material obtained in step S2 to the periphery of the honeycomb ceramic body, and then put it into a drying room at 40-70° C. for rapid drying for 2.0-4 hours to obtain a silicon carbide honeycomb ceramic body.

Citation Information

Patent Citations

  • Ceramic honeycomb structure skin coating

    CN102256600A

  • Non-fired high-hardness cordierite honeycomb ceramic skin and production method thereof

    CN105906367A

  • Circumferential coating material and circumferential coated honeycomb structure

    CN108623329A

  • Preparation method of skin-grafting pug for outer skin of honeycomb ceramic, and prepared skin-grafting pug

    CN111170709A

  • Low-thermal-expansion honeycomb ceramic peripheral coating material and preparation method thereof

    CN112608627A

Cited By

  • Splicing material, silicon carbide honeycomb ceramic, preparation method and application

    CN120903955A

  • Leather planting material, application and preparation method of silicon carbide honeycomb ceramic