Epoxidized natural rubber as well as preparation process and application thereof

The in-situ method of microfluidic field technology synthesize peroxyformic acid and epoxidize in natural rubber latex, combined with the gas-liquid separation design, solves the problems of many side reactions, long reaction time and low safety in traditional processes, and realizes the Epoxy natural rubber is efficient, safe and controllable, suitable for a variety of industries.

CN119080972APending Publication Date: 2024-12-06JIANGSU QIXIANG HIGH NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411357835.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing epoxidized natural rubber preparation process has problems such as many side reactions, long reaction time, low production efficiency, low safety and poor product batch stability. Especially the traditional kettle process has the risk of explosion and gas-liquid separation of materials. Uneven problem.

Method used

Using the microfluidic field technology in situ method, hydrogen peroxide and formic acid are synthesized in the first reactor of the microfluidic field by double-strand feed, and peroxyformic acid is synthesized with natural rubber in the second to fourth reactors of the microfluidic field. Emulsion reaction, combined with gas-liquid separation design, shortens reaction time, reduces side reactions, and improves reaction safety and product stability.

Benefits of technology

It greatly shortens the reaction time, improves the reaction safety and product stability, reduces the occurrence of side reactions, and realizes the efficient, safe and controllable preparation of epoxidized natural rubber, and the mechanical properties and epoxy values ​​of the product are controllable. Suitable for industries such as automobiles, energy and medical care.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080972A_ABST
    Figure CN119080972A_ABST
Patent Text Reader

Abstract

The invention discloses epoxidized natural rubber and a preparation process and application thereof.The preparation process of the epoxidized natural rubber adopts a micro-flow field technology in-situ method and comprises the following steps that peroxyformic acid is synthesized, the peroxyformic acid and natural rubber latex are pumped into a reactor for a reaction, and the epoxidized natural rubber is obtained; a gas-liquid separation tank is connected in series behind the reactor to discharge gas in a system in time, and after discharging, flocculation, washing and drying are performed to obtain the epoxidized natural rubber. According to the present invention, the epoxidized natural rubber is prepared by using the micro-flow field technology in-situ method, such that the reaction safety is improved, the reaction time is substantially shortened, the side reaction can be reduced, the product yield is improved, the equipment occupation area is small, the construction cost is saved, the continuous production can be achieved, and the product quality is stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of epoxidized natural rubber preparation, and in particular to epoxidized natural rubber and a preparation process and application thereof. Background Art

[0002] Natural rubber (NR) is a natural polymer compound with cis-1,4-polyisoprene as the main component. It is the most widely used general-purpose rubber and a renewable resource with an important strategic position. NR has many advantages, but due to its non-polar structure, it has poor affinity with polar fillers, poor reinforcement effect, low glass transition temperature, poor anti-slip performance, low air tightness and low oil resistance. The above disadvantages limit the application of NR in some special occasions, which makes the modification research of NR very important. In order to improve the performance of rubber and make more reasonable and efficient use of NR resources, scientific researchers have made many explorations. One of the directions is to epoxidize NR. Epoxidation modification can be carried out directly in situ in latex, with low cost and low pollution, and is more suitable for industrial production. Epoxidized natural rubber (ENR) is obtained by epoxidation modification of double bonds on natural rubber. The introduction of epoxy functional groups enables natural rubber to not only retain the characteristics of "strain induced crystallization" but also have excellent mechanical properties, and its wear resistance, oil resistance, adhesion and air tightness are all improved.

[0003] my country started research on epoxidized natural rubber relatively late, and mainly studied the blending performance of ENR with other materials. There was little research on the preparation process of ENR, which resulted in most commercially available ENR being imported from Malaysia and Thailand. Therefore, it is necessary to strengthen research on the preparation process of ENR. Currently, the preparation of ENR mostly adopts the in-situ method, that is, adding acid and hydrogen peroxide to the NR emulsion, and using the peroxy acid generated in the system to epoxidize the natural rubber. However, the traditional production process also has certain drawbacks.

[0004] First, in the process of preparing epoxidized natural rubber by in-situ method, as the reaction proceeds, side reactions also occur. When the degree of epoxidation is low, the acid in the system will hydrolyze with the epoxy group to generate diols and hydroxyl groups; when the degree of epoxidation is high, the epoxy group is easy to react with the adjacent epoxy group after ring opening to generate substituted furan structure. When the degree of epoxidation is high, crosslinking between the epoxy group and the epoxy rubber will also occur after the ring opening. Secondly, due to the long reaction time of the traditional kettle process, which requires 6-8h, the production efficiency is low, and there are risks such as explosion during the preparation and transfer of peroxides. The viscosity of the reaction system is relatively large. Whether it is a kettle reaction or a tubular reaction, hydrogen peroxide and peroxyformic acid will decompose to produce gas, resulting in the separation of the reaction liquid by gas, resulting in uneven mixing of materials, and the situation that the epoxy value is high and low between batches is prone to occur. There are many by-products such as ring opening and crosslinking, and there are defects such as poor product batch stability and low reaction safety. Therefore, it is urgent to develop a natural rubber epoxidation process with stable product performance, high efficiency and safety, so as to achieve the green, safe and controllable whole reaction, which is in line with the general direction of sustainable development. Summary of the invention

[0005] In view of the defects in the prior art, the present invention provides an epoxidized natural rubber and a preparation process and application thereof.

[0006] The present invention provides a preparation process of epoxidized natural rubber, which is prepared in situ by using microfluidic field technology, and comprises the following steps:

[0007] The hydrogen peroxide and formic acid are pumped from the raw material storage tank into the first microflow field reactor by using double feed to synthesize peroxyformic acid;

[0008] Pumping peroxyformic acid and natural rubber latex into a second microflow field reactor connected in series with the first reactor for reaction, and then discharging the materials into a first gas-liquid separation tank;

[0009] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and then enters the second gas-liquid separation tank after discharge, and the liquid phase enters the fourth microflow field reactor, and then flocculates, washes, and dries the discharged material to obtain epoxidized natural rubber;

[0010] The present invention uses microfluidic field technology to prepare epoxidized natural rubber in situ, which improves reaction safety, greatly shortens reaction time, and can reduce the occurrence of side reactions, such as preventing natural rubber from opening and breaking the chain under the action of formic acid for a long time, thereby preventing the natural rubber from losing its proper mechanical properties. In the conventional microchannel epoxidation reaction process, hydrogen peroxide and peracid decompose to produce gas, resulting in uneven gas-liquid distribution, inconsistent local acid concentration, and easy demulsification and clogging of the reactor. However, the present invention ensures that the reaction can proceed normally by adding structural turbulence and gas-liquid separation in the reaction design, and the equipment occupies a small area, saves construction costs, can be produced continuously, and has stable product quality.

[0011] In the present invention, the first reactor is used for preparing peroxyformic acid, the second reactor is used for synthesizing natural rubber with a lower epoxy value, the third reactor after gas-liquid separation can prepare natural rubber with an epoxy value of 25% or more, and the fourth reactor can also prepare products with a higher epoxy value, thereby obtaining natural rubber with an epoxy value of 35%-45%.

[0012] Furthermore, the solid content of the natural rubber emulsion is 5%-50%, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, and 50%. The solid content of the natural rubber emulsion affects the speed of the epoxidation reaction and the degree of epoxidation of the system. The higher the solid content, the faster the reaction speed and the higher the epoxidation degree of the system. The higher the solid content of the natural rubber emulsion, the greater the viscosity of the system, the worse the fluidity, and the worse the mass transfer effect in the pipeline. Therefore, the solid content of the natural rubber emulsion must be controlled within a certain range.

[0013] Furthermore, the natural rubber latex is prepared by the following steps: adding an emulsifier to a storage tank filled with water, stirring and dissolving at 20-40°C, adding natural latex, and stabilizing at 20-40°C for 0.5-1h to prepare the natural rubber latex; wherein the solid content of the natural latex is 15-61%, such as 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 61%, and the emulsifier is 0.5-5% of the amount of natural rubber in the natural latex, such as 0.5%, 1%, 2%, 3%, 4%, 5%;

[0014] The natural latex is fresh natural rubber latex or its concentrated product; the natural rubber emulsion is a premix obtained by processing natural latex.

[0015] Furthermore, the emulsifier is any one or more combinations of anionic or nonionic emulsifiers.

[0016] Furthermore, the emulsifier may be selected from the group consisting of secondary alcohol polyoxyethylene ether, dodecylphenol polyoxyethylene ether, carbonyl isomeric alcohol ethoxylate, sodium lauryl sulfate, sodium dodecyl diphenyl ether disulfonate, and sodium dodecyl polyoxyethylene ether sulfate, or a mixture of the two or more thereof.

[0017] Furthermore, in the first microfluidic field reactor, the reaction temperature is 10 to 90° C., preferably 40 to 60° C., and the residence time of the material in the pipeline is 3 to 20 minutes, preferably 10 minutes.

[0018] Furthermore, the concentration of the hydrogen peroxide is 10% to 90%, preferably 20% to 40%, and more preferably 30%.

[0019] Furthermore, the molar ratio of formic acid, hydrogen peroxide and natural rubber latex is (1-5):(3-8):4, and different ratios are selected according to the required epoxy value.

[0020] Furthermore, the pipelines of the second to fourth reactors of the microfluidic field are pipelines with an internal structure for enhanced mass and heat transfer or straight-through pipelines, and the inner diameter of the pipeline is 1 to 30 mm.

[0021] Furthermore, in the second to fourth reactors of the microflow field, the reaction temperature is 30-80°C. Too low a temperature will result in low reaction efficiency, while too high a reaction temperature will likely cause emulsifier demulsification and blockage of the pipeline over time. The reaction temperature is preferably 60°C, and the total residence time of the material in the pipeline is 9-30 minutes, preferably 10-20 minutes. Preferably, the material stays in the second to fourth reactors for 3-10 minutes respectively.

[0022] The present invention also provides epoxidized natural rubber obtained by the preparation process, wherein the epoxidized natural rubber has an epoxide value ranging from 5% to 45%, such as 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, and in particular, epoxidized natural rubber with an epoxide value of more than 25% can be prepared.

[0023] The present invention also provides the use of the epoxidized natural rubber in any one of the following:

[0024] (1) Seals, tires, and suspension systems in the automotive industry;

[0025] (2) Cables and oil pipelines in the energy industry;

[0026] (3) Medical device and drug packaging in the medical industry.

[0027] In summary, compared with the prior art, the present invention achieves the following technical effects:

[0028] (1) The epoxidized natural rubber preparation process of the present invention adopts a microchannel reactor to directly pump formic acid and hydrogen peroxide from a storage tank into the reactor to continuously prepare peroxyformic acid without storage. The online reaction volume is small, which greatly improves the reaction safety.

[0029] (2) The epoxidized natural rubber preparation process of the present invention adopts a microchannel reactor for continuous reaction and uses a pump to accurately control the feed sample, thereby avoiding human errors, improving product stability and saving labor costs;

[0030] (3) The epoxidized natural rubber preparation process of the present invention uses microfluidic field technology to greatly shorten the reaction time, shortening the reaction time from 6-8 hours in the kettle process to 20-30 minutes, reducing the probability of side reactions such as ring opening, crosslinking, and chain breaking of epoxidized natural rubber in a long acid environment, so that the product has a high molecular weight and good mechanical properties;

[0031] (4) The epoxidized natural rubber preparation process of the present invention can quickly separate the gas generated in the reaction by continuous gas-liquid separation, thereby improving the reactor utilization rate, improving the reaction efficiency, and reducing the risk of pipeline blockage, which has certain advantages over traditional kettle and tube reactions;

[0032] (5) The epoxidized natural rubber preparation process of the present invention can prepare epoxidized natural rubbers with different epoxy values ​​by adjusting parameters, and the epoxy value range is 5% to 45%;

[0033] (6) The epoxidized natural rubber preparation process of the present invention has a small reactor size and a small footprint, which can improve space utilization and enhance economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 This is a schematic diagram of the process for preparing epoxidized natural rubber according to the present invention;

[0036] Figure 2 The mechanism diagram of in-situ preparation of epoxidized natural rubber;

[0037] Figure 3 This is a diagram of the side reactions of natural rubber epoxidation in the traditional process;

[0038] Figure 4 For epoxidized natural rubber 1H NMR nuclear magnetic resonance hydrogen spectrum and peak position diagram;

[0039] Figure 5 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 5.6% in Example 1 of the present invention;

[0040] Figure 6 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 17.6% in Example 2 of the present invention;

[0041] Figure 7 is the DSC spectrum of the natural rubber of Example 2 of the present invention;

[0042] Figure 8 is the TGA spectrum of the natural rubber of Example 2 of the present invention;

[0043] Fig. 9 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 21.5% in Example 3 of the present invention;

[0044] Fig.10 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 23.8% in Example 4 of the present invention;

[0045] Fig.11 is the DSC spectrum of the natural rubber of Example 4 of the present invention;

[0046] Fig.12 is the TGA spectrum of the natural rubber of Example 4 of the present invention;

[0047] Fig.13 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 29.4% in Example 5 of the present invention;

[0048] Fig.14 is the DSC spectrum of the natural rubber of Example 5 of the present invention;

[0049] Fig.15 is the TGA spectrum of the natural rubber of Example 5 of the present invention;

[0050] Fig.16 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 32.6% in Example 6 of the present invention;

[0051] Fig.17 is the DSC spectrum of the natural rubber of Example 6 of the present invention;

[0052] Fig.18 is the TGA spectrum of the natural rubber of Example 6 of the present invention;

[0053] Fig.19 It is the nuclear magnetic resonance hydrogen spectrum of commercially available concentrated natural rubber latex;

[0054] Fig. 20This is a hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 16% prepared by the autoclave process in Comparative Example 1 of the present invention;

[0055] Fig.21 This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 25.8% prepared by the autoclave process in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0056] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only embodiments of a part of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0057] Example

[0058] The present invention is further described below in conjunction with specific examples and comparative examples. The following specific examples are all preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the following examples, and are particularly not limited to the types of the various component raw materials used in the following specific examples.

[0059] 1. Sources of Raw Materials in Examples and Comparative Examples

[0060] Unless otherwise specified, the raw materials of the examples and comparative examples of the present invention are commercially available.

[0061] 2. Various performance test methods

[0062] (1) Calculation of epoxy value: Calculated by the formula: epoxy value = epoxy group integral / (double bond integral + epoxy group integral) * 100%;

[0063] (2)DSC test: The test was conducted by differential scanning calorimetry with a temperature range of (-90)-200°C and a temperature ramp of 10°C / min.

[0064] (3) TGA test: The test was carried out using a thermogravimetric instrument with a temperature range of 30-800°C and a temperature ramp of 10°C / min.

[0065] Example 1

[0066] Example 1 A natural rubber having an epoxy value of 5.6% is prepared by an in-situ method using a microfluidic field technology, comprising the following steps:

[0067] Add 1.5 g of secondary alcohol polyoxyethylene ether emulsifier (5% of the amount of natural rubber) to a storage tank containing 400 g of water, stir and dissolve at 30° C., then add 200 g of natural latex with a solid content of 15%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 5%;

[0068] A double feed was used to pump 15% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 1:6. The material synthesized peroxyformic acid at a temperature of 40°C with a retention time of 3 minutes.

[0069] Pumping peroxyformic acid and natural rubber latex into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber latex to formic acid to be 4:1, the material synthesizes epoxidized natural rubber at a temperature of 50°C, the retention time is 4 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0070] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and after the material is discharged, it enters the second gas-liquid separation tank, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the material in the third to fourth reactors is 50° C., and the residence time is 4 minutes. After the material is stably discharged, it is flocculated, washed, and dried to obtain an epoxidized natural rubber with an epoxy value of 5.6%;

[0071] Figure 1 The present invention is a schematic diagram of the process flow of preparing epoxidized natural rubber, wherein storage tank 1 is a formic acid raw material storage tank, storage tank 2 is a hydrogen peroxide raw material storage tank, storage tank 3 is a natural rubber emulsion raw material storage tank, M1, M2, and M3 correspond to the plunger pumps of storage tanks 1, 2, and 3, respectively, R101 corresponds to the first microflow field reactor, which is used to prepare peroxyformic acid, R102, R103, and R104 correspond to the second to fourth microflow field reactors, which are used to prepare epoxidized natural rubber, and G1 and G2 are gas-liquid separation tanks, which are used to separate the gas generated in the reaction;

[0072] Figure 5 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 5.6% in Example 1.

[0073] Example 2

[0074] Example 2 A natural rubber having an epoxy value of 17.6% is prepared by an in-situ method using microfluidic technology, comprising the following steps:

[0075] Add 2.4 g of dodecylphenol polyoxyethylene ether emulsifier (4.0% of the amount of natural rubber) to a storage tank containing 200 g of water, stir and dissolve at 30° C., then add 200 g of natural rubber latex with a solid content of 30%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 15%;

[0076] A double feed was used to pump 25% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 1:5. The materials synthesized peroxyformic acid at a temperature of 40°C with a retention time of 5 minutes.

[0077] Pumping peroxyformic acid and natural rubber latex into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber latex to formic acid to be 4:1, the material synthesizes epoxidized natural rubber at a temperature of 50°C, the retention time is 4 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0078] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and then enters the second gas-liquid separation tank after discharge, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the materials in the third and fourth reactors is 50° C., and the residence time is 4 minutes. After stable discharge, the epoxidized natural rubber with an epoxy value of 17.6% is obtained by flocculation, washing, and drying.

[0079] Figure 6 This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 17.6% in Example 2;

[0080] Figure 7 is the DSC spectrum of the natural rubber of Example 2;

[0081] Figure 8 This is the TGA spectrum of the natural rubber of Example 2.

[0082] Example 3

[0083] Example 3 A natural rubber having an epoxy value of 21.5% is prepared by an in-situ method using microfluidic technology, comprising the following steps:

[0084] Add 1.8 g of sodium dodecyl sulfate emulsifier (1.5% of the amount of natural rubber) to a storage tank containing 200 g of water, stir and dissolve at 30° C., then add 200 g of natural rubber latex with a solid content of 60%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 30%;

[0085] A double feed was used to pump 30% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 2:5. The materials synthesized peroxyformic acid at a temperature of 50°C with a retention time of 6 minutes.

[0086] Pumping peroxyformic acid and natural rubber latex into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber latex to hydrogen peroxide to be 4:5, the material synthesizes epoxidized natural rubber at a temperature of 60°C, the retention time is 4 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0087] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and then enters the second gas-liquid separation tank after discharge, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the materials in the third and fourth reactors is 60° C., and the residence time is 4 minutes. After stable discharge, the epoxidized natural rubber with an epoxy value of 21.5% is obtained by flocculation, washing, and drying.

[0088] Fig. 9 This is the nuclear magnetic resonance hydrogen spectrum of the natural rubber with an epoxy value of 21.5% in Example 3.

[0089] Example 4

[0090] Example 4 A natural rubber having an epoxy value of 23.8% is prepared by an in-situ method using microfluidic technology, comprising the following steps:

[0091] Add 4.2 g of sodium dodecyl diphenyl ether disulfonate emulsifier (3.5% of the amount of natural rubber) to a storage tank containing 100 g of water, stir and dissolve at 30° C., then add 200 g of natural rubber latex with a solid content of 60%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 40%;

[0092] A double feed was used to pump 30% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 3:5. The material synthesized peroxyformic acid at a temperature of 40°C with a retention time of 6 minutes.

[0093] Pumping peroxyformic acid and natural rubber latex into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber latex to formic acid to be 4:3, the material synthesizes epoxidized natural rubber at a temperature of 60°C, the retention time is 5 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0094] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and then enters the second gas-liquid separation tank after discharge, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the materials in the third and fourth reactors is 60° C., and the residence time is 5 minutes. After stable discharge, the epoxidized natural rubber with an epoxy value of 23.8% is obtained by flocculation, washing, and drying.

[0095] Fig.10This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 23.8% in Example 4;

[0096] Fig.11 is the DSC spectrum of the natural rubber of Example 4;

[0097] Fig.12 This is the TGA spectrum of the natural rubber of Example 4.

[0098] Example 5

[0099] Example 5 A natural rubber having an epoxy value of 29.4% is prepared by an in-situ method using microfluidic technology, comprising the following steps:

[0100] Add 1.8 g of secondary alcohol polyoxyethylene ether emulsifier (1.5% of the amount of natural rubber) to a storage tank containing 65 g of water, stir and dissolve at 30° C., then add 200 g of natural latex with a solid content of 60%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 45%;

[0101] A double feed was used to pump 30% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 2:3. The materials synthesized peroxyformic acid at a temperature of 40°C with a retention time of 5 minutes.

[0102] Pumping peroxyformic acid and natural rubber emulsion into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber emulsion to hydrogen peroxide to be 2:3, the material synthesizes epoxidized natural rubber at a temperature of 50°C, the retention time is 6 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0103] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and then enters the second gas-liquid separation tank after discharge, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the materials in the third and fourth reactors is 50° C., and the residence time is 6 minutes. After stable discharge, the epoxidized natural rubber with an epoxy value of 29.4% is obtained by flocculation, washing, and drying.

[0104] Fig.13 This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 29.4% in Example 5;

[0105] Fig.14 is the DSC spectrum of the natural rubber of Example 5;

[0106] Fig.15 This is the TGA spectrum of the natural rubber of Example 5.

[0107] Example 6

[0108] Example 6 A natural rubber having an epoxy value of 32.6% is prepared by an in-situ method using microfluidic technology, comprising the following steps:

[0109] Add 4.2 g of secondary alcohol polyoxyethylene ether emulsifier (3.5% of the amount of natural rubber) to a storage tank containing 50 g of water, stir and dissolve at 30° C., then add 200 g of natural latex with a solid content of 60%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 48%;

[0110] A double feed was used to pump 30% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 2:3. The materials synthesized peroxyformic acid at a temperature of 50°C with a retention time of 8 minutes.

[0111] Pumping peroxyformic acid and natural rubber emulsion into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber emulsion to hydrogen peroxide to be 2:3, the material synthesizes epoxidized natural rubber at a temperature of 65°C, the retention time is 6 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0112] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor, and then enters the second gas-liquid separation tank after discharge, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the materials in the third and fourth reactors is 65° C., and the residence time is 6 minutes. After stable discharge, the epoxidized natural rubber with an epoxy value of 32.6% is obtained by flocculation, washing, and drying.

[0113] Fig.16 This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 32.6% in Example 6;

[0114] Fig.17 is the DSC spectrum of the natural rubber of Example 6;

[0115] Fig.18 This is the TGA spectrum of the natural rubber of Example 6.

[0116] Example 7

[0117] Example 7 A natural rubber having an epoxy value of 45.0% is prepared by an in-situ method using microfluidic technology, comprising the following steps:

[0118] Add 3.0 g of sodium dodecyl sulfate emulsifier (2.5% of the amount of natural rubber) to a storage tank containing 40 g of water, stir and dissolve at 30° C., then add 200 g of natural rubber latex with a solid content of 60%, and stabilize for 0.5 hours to obtain a natural rubber latex with a solid content of 50%;

[0119] A double feed was used to pump 30% hydrogen peroxide and formic acid from a raw material storage tank into the first microflow field reactor, and a metering pump was used to adjust the molar ratio of formic acid to hydrogen peroxide to 2:3. The materials synthesized peroxyformic acid at a temperature of 40°C with a retention time of 10 minutes.

[0120] Pumping peroxyformic acid and natural rubber emulsion into a second microflow field reactor connected in series with the first reactor for reaction, controlling the molar ratio of natural rubber emulsion to hydrogen peroxide to be 2:3, the material synthesizes epoxidized natural rubber at a temperature of 65°C, the retention time is 6 minutes, and the material enters the first gas-liquid separation tank after discharge;

[0121] The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor. After discharge, it enters the second gas-liquid separation tank, and the liquid phase enters the fourth microflow field reactor. The reaction temperature of the material in the third to fourth reactors is 65°C, and the residence time is 6 minutes. After stable discharge, flocculation, washing and drying are performed to obtain epoxidized natural rubber with an epoxy value of 45.0%.

[0122] Comparative Example 1

[0123] Comparative Example 1 is a process for preparing natural rubber with an epoxy value of 15% by a kettle process, comprising the following steps:

[0124] 1.8 g of OP-10 emulsifier was mixed with 100 g of water, and stirred at 30°C to dissolve. 100 g of 60% natural latex was weighed and added to a 1 L reaction flask. The dissolved OP-10 solution was added to the flask and mixed with the latex for emulsification. After stabilization for 0.5 h, the temperature was raised to 40°C. 10 g of formic acid was slowly dripped into the reaction flask drop by drop. After the addition was completed, 75 g of 30% hydrogen peroxide was slowly dripped into the latex. The addition time was about 30 min. After the hydrogen peroxide was added, the temperature was raised to 50°C for 6 h. After the reaction was completed, ethanol was used for flocculation, washing, and drying to obtain the finished product.

[0125] Fig. 20 This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 16% prepared by the autoclave process in Comparative Example 1.

[0126] Comparative Example 2

[0127] Comparative Example 2 is a process for preparing natural rubber with an epoxy value of 25% by a kettle process, comprising the following steps:

[0128] 1.8 g of OP-10 emulsifier was mixed with 100 g of water, and stirred at 30°C to dissolve. 100 g of 60% natural latex was weighed and added to a 1L reaction flask. The dissolved OP-10 solution was added to the flask and mixed with the latex for emulsification. After stabilization for 0.5 h, the temperature was raised to 40°C. 10 g of formic acid was slowly dripped into the reaction flask drop by drop. After the addition was completed, 100 g of 30% hydrogen peroxide was slowly dripped into the latex for about 30 min. After the hydrogen peroxide was added, the temperature was raised to 50°C and kept for 8 h. After the reaction was completed, ethanol was used for flocculation, washing, and drying to obtain the finished product.

[0129] Fig.21 This is the hydrogen nuclear magnetic resonance spectrum of the natural rubber with an epoxy value of 25% prepared by the kettle process in Comparative Example 2.

[0130] Table 1 Technical effects of embodiments and comparative examples

[0131]

[0132] Examples 1-7 all adopt the microflow field technology in-situ method to prepare epoxidized natural rubber, adopt a microflow field reactor for continuous reaction, utilize the microscale effect to synthesize peroxyformic acid in the first reactor, and enter the second reactor for reaction after the synthesis of peroxyformic acid is completed, thereby avoiding the risks of storage and transportation; the gas in the system is discharged through the gas-liquid separation tank to improve the reaction efficiency; the reactor is small in size and occupies a small area, making the entire reaction green, safe, and controllable, which is in line with the general direction of sustainable development; and the epoxide value of the epoxidized natural rubber obtained can be controlled by the molar ratio of the raw materials in the reaction process, and the reaction yield is high. It is a new preparation process for epoxidized natural rubber.

[0133] It can be seen from the TGA spectrum in the accompanying drawings that the initial decomposition temperature of the epoxy natural rubber prepared by the present invention is above 340°C, and it has high thermal stability; it can be seen from the DSC spectrum that the Tg of the epoxy natural rubber prepared by the present invention increases significantly with the increase of the epoxy value, which shows that the epoxy natural rubber prepared by the preparation method of the present invention has high stability.

[0134] Comparative Example 1-2 adopts a kettle process to prepare epoxy natural rubber. Since formic acid is directly dispersed in the latex system in the kettle process, the probability of contact with hydrogen peroxide becomes smaller, so the rate of generating peroxyformic acid is low, resulting in a slower rate of generating epoxy natural rubber.

[0135] Based on the test data of the reaction time in Table 1, the preparation of epoxidized natural rubber by the process of Examples 1-7 has obvious advantages over the comparative example and can effectively meet the high standards of customers and the market.

[0136] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for preparing epoxidized natural rubber, characterized in that: The in-situ preparation method using microfluidic field technology includes the following steps: The hydrogen peroxide and formic acid are pumped from the raw material storage tank into the first microflow field reactor by using double feed to synthesize peroxyformic acid; Pumping peroxyformic acid and natural rubber latex into a second microflow field reactor connected in series with the first reactor for reaction, and then discharging the materials into a first gas-liquid separation tank; The gas generated in the reaction is discharged through the first gas-liquid separation tank, and the liquid after gas-liquid separation is pumped into the third microflow field reactor. After discharge, it enters the second gas-liquid separation tank, and the liquid phase enters the fourth microflow field reactor. After discharge, it is flocculated, washed, and dried to obtain epoxidized natural rubber.

2. The preparation process according to claim 1, characterized in that: The solid content of the natural rubber latex is 5%-50%.

3. The preparation process according to claim 2, characterized in that: The natural rubber emulsion is prepared by the following steps: adding an emulsifier into a storage tank filled with water, stirring and dissolving at 20-40°C, adding natural latex, and stabilizing at 20-40°C for 0.5-1h to prepare the natural rubber emulsion; wherein the solid content of the natural latex is 15-61%, and the emulsifier is 0.5-5% of the amount of natural rubber in the natural latex.

4. The preparation process according to claim 3, characterized in that: The emulsifier is any one or more combinations of anionic or nonionic emulsifiers.

5. The preparation process according to claim 1, characterized in that: In the first microfluidic field reactor, the reaction temperature is 10-90° C., and the residence time of the material in the pipeline is 3-20 minutes.

6. The preparation process according to claim 1, characterized in that: The molar ratio of formic acid, hydrogen peroxide and natural rubber latex is (1-5):(3-8):

4.

7. The preparation process according to claim 1, characterized in that: The pipelines of the second to fourth reactors of the microfluidic field are pipelines with an internal structure for enhanced mass and heat transfer or straight-through pipelines, and the inner diameter of the pipeline is 1 to 30 mm.

8. The preparation process according to claim 1, characterized in that: In the second to fourth reactors of the microfluidic field, the reaction temperature is 30-80° C., the total residence time of the material in the pipeline is 9-30 minutes, and the material stays in the second to fourth reactors for 3-10 minutes respectively.

9. The epoxidized natural rubber obtained by the preparation process according to any one of claims 1 to 8, characterized in that: The epoxy value of the epoxidized natural rubber ranges from 5% to 45%.

10. Use of the epoxidized natural rubber according to claim 9 in any of the following: (1) Seals, tires, and suspension systems in the automotive industry; (2) Cables and oil pipelines in the energy industry; (3) Medical device and drug packaging in the medical industry.