Polyaldehyde ester prepared by copolymerization of formaldehyde and anhydride and preparation method thereof
By screening cyclic anhydride and catalyst, polyaldehyde esters with AB and ABB links were prepared, which solved the problem of formaldehyde homopolymerization stability and recycling and reuse, achieved the diversity and stability of polymer structure, and met the low-carbon Economic demand.
Patent Information
- Application Number
- CN202310653439.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively regulate the polymer main chain structure, especially the homopolymerization reaction of formaldehyde, and the recycling and reuse of formaldehyde is difficult, which affects its application.
By screening suitable cyclic anhydride monomers for alternating copolymerization with formaldehyde, using Lewis acid or protic acid as catalysts, polyaldehyde esters with fully alternating structures of AB links and ABB links were prepared to significantly inhibit the homopolymerization of formaldehyde. Control the structure of the polymer.
The formaldehyde copolymers with various structures were successfully prepared, which significantly inhibited the homopolymerization reaction of formaldehyde, achieved the diversity and stability of polyaldehyde esters, and no formaldehyde homopolymerization links were detected, satisfying the low-carbon economy of polymer materials application requirements.
Smart Images

Figure CN119081041A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a polyaldehyde ester prepared by copolymerization of formaldehyde and acid anhydride and a preparation method thereof. Background Art
[0002] The rapid development of industrialization has improved people's lives while also bringing new challenges. The development and utilization of a large number of petroleum-based materials has caused people to worry about energy depletion. At the same time, the large-scale development and utilization of fossil fuels produces a large amount of carbon dioxide, which is one of the main causes of global warming. In order to cope with energy problems, the world is calling for "low-carbon" development. In order to meet this challenge, it is urgent to develop new polymer materials and synthesis methods, and use carbon-rich polymers for "carbon fixation" and reuse.
[0003] Polymers are macromolecules formed by bonding repeating units, and the difference in repeating units will greatly affect the properties of polymers. The current copolymerization is mainly random, block, grafted, and alternating copolymerization. It is difficult to strictly and finely adjust the main chain structure of the polymer, and relatively few studies have been conducted (Macromolecules 2020, 53, 9869-9877). The copolymerization of epoxy and carbon dioxide is an ideal method that meets the requirements of this standard for environmental friendliness and atom economy. The prepared polymer has good performance and has been widely studied by scholars at home and abroad. Compared with carbon dioxide, formaldehyde is also a carbon-rich carbon-monomer, but the recycling and reuse of formaldehyde has always been a serious issue. The homopolymerization of formaldehyde is a reversible equilibrium reaction. There is a balance between trioxymethylene and polyoxymethylene. In order to improve its stability for further application, cyclic acetals or cyclic ethers are often added as comonomers. Due to the lower homopolymerization activation barrier, formaldehyde is more inclined to undergo homopolymerization thermodynamically, so developing new methods to synthesize formaldehyde copolymers is a meaningful but difficult challenge. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention discloses several oxymethylene copolymers with different structures, especially discloses for the first time a polyaldehyde ester with a fully alternating structure of AB chain segments and a polyaldehyde ester with ABB chain segments with a clear structure.
[0005] The specific technical solutions are as follows:
[0006] A polyaldehyde ester prepared by copolymerization of formaldehyde and acid anhydride, the general structural formula of which is shown in the following formulas (I) to (VI):
[0007]
[0008] In the formula, n1 to n6 are independently selected from integers of 0 to 1000, and m1 to m6 are independently selected from integers of 0 to 1000.
[0009] Preferably, n1-n6 are independently selected from integers of 0-100, and m1-m6 are independently selected from integers of 0-100.
[0010] For the general structural formulas (II) to (IV), by specially screening the types of anhydride monomers and catalysts, polyaldehyde esters with a fully alternating structure having only AB chain segments can be prepared, that is, in the above-mentioned general structural formulas, m2 to m4 are all equal to 0.
[0011] For the general structural formulas (V) to (VI), polyaldehyde esters having only ABB segments can be prepared by special screening of the types of anhydride monomers and catalysts, that is, in the above general structural formulas, n5 to n6 are all equal to 0.
[0012] The present invention also discloses a method for preparing the polyaldehyde ester, comprising:
[0013] The polyaldehyde ester is prepared by using formaldehyde and / or trioxymethylene and cyclic anhydride as raw materials and Lewis acid or protonic acid as catalyst through alternating copolymerization;
[0014] The cyclic anhydride is selected from one or more of SA (succinic anhydride), GA (glutaric anhydride), 3-MGA (3-methylglutaric anhydride), 3-iBuGA (3-isobutylglutaric anhydride), DGA (diglycolic anhydride), and TDGA (thiodiglycolic anhydride).
[0015] In the preparation method of the present invention, formaldehyde and / or trioxymethylene is used as a raw material and cyclic acid anhydride is used as another raw material to carry out copolymerization reaction.
[0016] Since formaldehyde is a gas, it is preferable to use solid trioxymethylene as a raw material.
[0017] The Lewis acid is selected from one or more of BF3, B(C6F5)3, InCl3, InBr3, SnCl4, AlCl3, SbCl5, PF5, CF3SO3Et, and Ph3CPF6;
[0018] The protonic acid is selected from one or more of HBF4, HClO4, HN(SO2CF3)2, HN(SO2)2(CF2)3, CF3COOH, CF3SO4H, FSO4H and concentrated sulfuric acid.
[0019] Preferably, the molar ratio of formaldehyde to cyclic anhydride is 0.1 to 10:1; more preferably 0.5 to 2.0:1; and more preferably 1:1.
[0020] Preferably, the molar ratio of trioxymethylene to cyclic anhydride is 0.1 to 10:3; more preferably 0.5 to 2.0:3; and more preferably 1:3.
[0021] Preferably, the molar ratio of the catalyst to the cyclic anhydride is 1:10 to 2000, more preferably 1:20 to 2000, more preferably 1:100 to 2000, and even more preferably 1:500 to 2000. As the molar ratio is continuously optimized, the molecular weight of the prepared polyaldehyde ester increases continuously.
[0022] Preferably, the alternating copolymerization is carried out at 80-120° C. under autogenous pressure.
[0023] It has been found through experiments that when the cyclic anhydride is selected from SA, no matter which catalyst is used, the random copolymers prepared are all containing AB and ABB chain segments.
[0024] When the cyclic anhydride is selected from one or more of GA, 3-MGA, and 3-iBuGA, and the catalyst is selected from protonic acid, the prepared copolymer is a fully alternating copolymer having only AB segments;
[0025] However, if the protonic acid is replaced by Lewis acid, the fully alternating copolymer cannot be prepared.
[0026] Preferably, the protonic acid is selected from one or more of concentrated H2SO4, HClO4, HN(SO2CF3)2, and HN(SO2)2(CF2)3.
[0027] When the cyclic anhydride is selected from DGA and / or TDGA, and the catalyst is selected from protonic acid, the copolymer prepared has only ABB segments;
[0028] However, if the protonic acid is replaced by a Lewis acid, a random copolymer containing AB and ABB segments is obtained instead of a copolymer with a well-defined ABB segment.
[0029] Preferably, the protonic acid is selected from one or more of concentrated H2SO4, HClO4, HN(SO2CF3)2, and HN(SO2)2(CF2)3.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The invention significantly inhibits the homopolymerization reaction of formaldehyde by screening suitable cyclic anhydride monomers for copolymerization with formaldehyde, thereby preparing formaldehyde copolymers with various structures, and no formaldehyde homopolymer chain segments are detected in the copolymer products.
[0032] The present invention also controllably prepares polyaldehyde esters with a fully alternating structure of AB chain segments and polyaldehyde esters with ABB chain segments with a clear structure after screening the cyclic anhydride monomers in the catalyst system. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1The polyaldehyde ester prepared in Example 1 1 H NMR spectrum;
[0034] Figure 2 The polyaldehyde ester prepared in Example 1 13 C NMR spectrum;
[0035] Figure 3 The polyaldehyde ester prepared in Example 3 1 H NMR spectrum;
[0036] Figure 4 The polyaldehyde ester prepared in Example 3 13 C NMR spectrum;
[0037] Figure 5 The polyaldehyde ester prepared in Example 7 1 H NMR spectrum;
[0038] Figure 6 The polyaldehyde ester prepared in Example 7 13 C NMR spectrum;
[0039] Figure 7 The polyaldehyde ester prepared in Example 12 1 H NMR spectrum;
[0040] Figure 8 The polyaldehyde ester prepared in Example 12 13 C NMR spectrum;
[0041] Fig. 9 The polyaldehyde ester prepared in Example 13 1 H NMR spectrum;
[0042] Fig.10 The polyaldehyde ester prepared in Example 13 13 C NMR spectrum;
[0043] Fig.11 The polyaldehyde ester prepared in Example 14 1 H NMR spectrum;
[0044] Fig.12 The polyaldehyde ester prepared in Example 14 13 C NMR spectrum;
[0045] Fig.13 The polyaldehyde ester prepared in Example 15 1 H NMR spectrum;
[0046] Fig.14 The polyaldehyde ester prepared in Example 15 13 C NMR spectrum;
[0047] Fig.15 The polyaldehyde ester prepared in Example 16 1 H NMR spectrum. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.
[0049] Example 1 Formaldehyde / succinic anhydride alternate copolymerization to form polyaldehyde ester
[0050] Before the polymerization reaction, remove moisture from a 10mL Shrek tube at 110°C for 2h and cool to room temperature in a glove box; add a certain mass of concentrated H2SO4 (98wt%), formaldehyde, succinic anhydride and 1mL of dichloromethane to the Shrek tube in sequence. The molar ratio of concentrated H2SO4 / formaldehyde / succinic anhydride is 3 / 100 / 300. React at 100°C under autogenous pressure for 0.5h. After the reaction is completed, dissolve the crude product with dichloromethane, then precipitate the polymer in a mixture of 100mL of methanol / sodium phenolate (sodium phenolate molar concentration is 5%), repeat washing three times, and vacuum dry to constant weight. The structural formula of the product is as follows, where n1 is 13 and m1 is 6:
[0051]
[0052] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0053] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 1 As shown, 13 CNMR spectrum Figure 2 Observation Figure 1 and Figure 2 It can be seen that the main chain segments in the polymer are AB and ABB structural chain segments, and no homopolymer chain segments of formaldehyde are generated, indicating that the product is a random copolymer containing AB and ABB chain segments.
[0054] Example 2 Formaldehyde / succinic anhydride alternate copolymerization to form polyaldehyde ester
[0055] Before the polymerization reaction, remove moisture from a 10mL Shrek tube at 110°C for 2 hours and cool to room temperature in a glove box; add a certain amount of BF3, trioxymethylene, succinic anhydride and 1mL of dichloromethane to the Shrek tube in sequence. The molar ratio of BF3 / formaldehyde / succinic anhydride is 3 / 100 / 300. React at 100°C under autogenous pressure for 0.5 hours. After the reaction is completed, dissolve the crude product with dichloromethane, and then precipitate the polymer in a mixture of 100mL of methanol / sodium phenolate (sodium phenolate molar concentration is 5%), repeat washing three times, and vacuum dry to constant weight.
[0056] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0057] Further characterization by H-NMR and C-NMR showed that the main chain segments in the polyaldehyde ester polymer prepared in this example were AB and ABB structure chains, and no homopolymer chain segments of formaldehyde were generated, indicating that the product was a random copolymer containing AB and ABB chains.
[0058] Example 3 Alternating copolymerization of formaldehyde / glutaric anhydride to form fully alternating polyaldehyde esters
[0059] Before the polymerization reaction, remove moisture from a 10mL Shrek tube at 110°C for 2h and cool to room temperature in a glove box; add a certain mass of concentrated H2SO4 (98wt%), trioxymethylene, glutaric anhydride and 1mL of dichloromethane to the Shrek tube in sequence. The molar ratio of concentrated H2SO4 / trioxymethylene / glutaric anhydride is 3 / 100 / 300. React at 100°C under autogenous pressure for 0.5h. After the reaction is completed, dissolve the crude product with dichloromethane, then precipitate the polymer in a mixture of 100mL of methanol / sodium phenolate (sodium phenolate molar concentration is 5%), repeat washing three times, and vacuum dry to constant weight. The structural formula of the product is as follows, where n2 is 100:
[0060]
[0061] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0062] The fully alternating polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 3 As shown, 13 C NMR spectrum Figure 4 Observation Figure 3 and Figure 4 It can be seen that there are no peaks corresponding to formaldehyde homopolymerization links and ABB links formed by double insertion of formaldehyde in the figure, indicating that the obtained product is a completely alternating link structure containing only AB.
[0063] Examples 4-6 Alternating copolymerization of formaldehyde / glutaric anhydride to form fully alternating polyaldehyde esters
[0064] The preparation process is basically the same as that in Example 3, except that the catalyst is replaced with equimolar amounts of HClO4 (70wt%), HN(SO2CF3)2, and HN(SO2)2(CF2)3 in sequence.
[0065] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0066] Further characterization by H-NMR and C-NMR spectra revealed that no peaks corresponding to homopolymerized formaldehyde chains or ABB chains formed by double insertion of formaldehyde were observed in the polymers prepared in each example, indicating that the obtained products all contained only AB complete alternating chain structures.
[0067] Example 7 Formaldehyde / glutaric anhydride alternating copolymerization to form polyaldehyde ester
[0068] The preparation process is basically the same as that in Example 3, except that the catalyst is replaced with an equal molar amount of BF3. The structural formula of the product is as follows, where n2 is 53 and m2 is 23:
[0069]
[0070] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0071] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 5 As shown, 13 CNMR spectrum Figure 6 Observation Figure 5 and Figure 6 It can be seen that the main chain segments in the polymer are AB and ABB structural chain segments, and no homopolymer chain segments of formaldehyde are generated, indicating that the product is a random copolymer containing AB and ABB chain segments.
[0072] Example 8 Formaldehyde / glutaric anhydride alternating copolymerization to form polyaldehyde ester
[0073] The preparation process is basically the same as that in Example 3, except that the catalyst is replaced with an equimolar amount of B(C6F5)3.
[0074] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0075] Further characterization by H-NMR and C-NMR showed that the main chain segments in the polyaldehyde ester polymer prepared in this example were AB and ABB structure chains, and no homopolymer chain segments of formaldehyde were generated, indicating that the product was a random copolymer containing AB and ABB chains.
[0076] Example 9 Alternating copolymerization of formaldehyde / glutaric anhydride to form fully alternating polyaldehyde esters
[0077] The preparation process is basically the same as that in Example 3, except that the molar ratio of concentrated H2SO4 / trioxymethylene / glutaric anhydride is replaced with 3:20:60.
[0078] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0079] Further characterization by H-NMR and C-NMR spectra revealed that the polyaldehyde ester prepared in this embodiment did not contain any formaldehyde homopolymer chain segments, nor any peaks corresponding to ABB chain segments formed by double insertion of formaldehyde, indicating that the obtained product was a completely alternating chain segment structure containing only AB.
[0080] Example 10 Alternating copolymerization of formaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0081] The preparation process is basically the same as that in Example 3, except that the molar ratio of concentrated H2SO4 / trioxymethylene / glutaric anhydride is replaced with 3:500:1500, and the polymerization time is replaced with 3 h.
[0082] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0083] Further characterization by H-NMR and C-NMR spectra revealed that the polyaldehyde ester prepared in this embodiment did not contain any formaldehyde homopolymer chain segments, nor any peaks corresponding to ABB chain segments formed by double insertion of formaldehyde, indicating that the obtained product was a completely alternating chain segment structure containing only AB.
[0084] Example 11 Alternating copolymerization of formaldehyde / glutaric anhydride to form fully alternating polyaldehyde ester
[0085] The preparation process is basically the same as that in Example 3, except that the molar ratio of concentrated H2SO4 / trioxymethylene / glutaric anhydride is replaced with 3:2000:6000, and the polymerization time is replaced with 12 h.
[0086] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0087] Further characterization by H-NMR and C-NMR spectra revealed that the polyaldehyde ester prepared in this embodiment did not contain any formaldehyde homopolymer chain segments, nor any peaks corresponding to ABB chain segments formed by double insertion of formaldehyde, indicating that the obtained product was a completely alternating chain segment structure containing only AB.
[0088] Example 12 Alternating copolymerization of formaldehyde / 3-isobutylglutaric anhydride to form fully alternating polyaldehyde ester
[0089] The preparation process is basically the same as that in Example 3, except that the cyclic anhydride is replaced by an equal molar amount of 3-isobutylglutaric anhydride. The structural formula of the product is as follows, where n4 is 23:
[0090]
[0091] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0092] The fully alternating polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Figure 7 As shown, 13 C NMR spectrum Figure 8 Observation Figure 7 and Figure 8 It can be seen that there is no formaldehyde homopolymer chain segment in the polymer, and there is no peak corresponding to the ABB chain segment formed by the double insertion of formaldehyde, indicating that the obtained product is a completely alternating chain segment structure containing only AB.
[0093] Example 13 Alternating copolymerization of formaldehyde / 3-methylglutaric anhydride to form fully alternating polyaldehyde ester
[0094] The preparation process is basically the same as that in Example 3, except that the cyclic anhydride is replaced by an equal molar amount of 3-methylglutaric anhydride. The structural formula of the product is as follows, wherein n3 is 55:
[0095]
[0096] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0097] The fully alternating polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig. 9 As shown, 13 C NMR spectrum Fig.10 Observation Fig. 9 and Fig.10 It can be seen that there are no formaldehyde homopolymerization chains in the main chains of the polymer, and there are no peaks corresponding to the ABB chains formed by double insertion of formaldehyde, indicating that the obtained product is a completely alternating chain structure containing only AB.
[0098] Example 14 Formaldehyde / diglycolic anhydride alternating copolymerization to synthesize ABB sequence polyaldehyde ester
[0099] Before the polymerization reaction, remove moisture from a 10mL Shrek tube at 110°C for 2h and cool to room temperature in a glove box; add a certain mass of concentrated H2SO4, trioxymethylene, diglycolic anhydride and 1mL of dichloromethane to the Shrek tube in sequence. The molar ratio of concentrated H2SO4 / trioxymethylene / diglycolic anhydride is 3 / 100 / 300. React at 80°C under autogenous pressure for 20min. After the reaction, dissolve the crude product with dichloromethane, then precipitate the polymer in a mixture of 100mL of methanol / sodium phenolate (sodium phenolate molar concentration is 5%), repeat washing three times, and vacuum dry to constant weight. The structural formula of the product is as follows, where m5 is 19:
[0100]
[0101] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0102] The fully alternating polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig.11 As shown, 13 C NMR spectrum Fig.12 Observation Fig.11 and Fig.12 It can be seen that each polyaldehyde ester chain link is connected to a formaldehyde chain link, indicating that the obtained product has a clear ABB sequence structure.
[0103] Example 15 Formaldehyde / thiodiglycolic anhydride alternating copolymerization to synthesize ABB sequence polyaldehyde ester
[0104] Before the polymerization reaction, remove moisture from a 10mL Shrek tube at 110°C for 2 hours and cool to room temperature in a glove box; add a certain mass of H2SO4, trioxymethylene, thiodiglycolic anhydride and 1mL of dichloromethane to the Shrek tube in sequence. The molar ratio of H2SO4 / formaldehyde / thiodiglycolic anhydride is 3 / 100 / 300. React at 80°C under autogenous pressure for 0.5 hours. After the reaction is completed, dissolve the crude product with dichloromethane, then precipitate the polymer in a mixture of 100mL of methanol / sodium phenolate (sodium phenolate molar concentration is 5%), repeat washing three times, and vacuum dry to constant weight. The structural formula of the product is as follows, where m6 is 13:
[0105]
[0106] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0107] The fully alternating polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig.13 As shown, 13 C NMR spectrum Fig.14 Observation Fig.13 and Fig.14 It can be seen that each polyaldehyde ester chain link is connected to a formaldehyde chain link, indicating that the obtained product has a clear ABB sequence structure.
[0108] Example 16 Alternating copolymerization of formaldehyde / diglycolic anhydride to form polyaldehyde ester
[0109] The preparation process is basically the same as that in Example 14, except that the catalyst is replaced with an equimolar amount of B(C6F5)3. The structural formula of the product is as follows, where n5 is 2 and m5 is 6:
[0110]
[0111] The molecular weight and molecular weight distribution of the polymer were determined by gel chromatography. The test results are shown in Table 1.
[0112] The polyaldehyde ester prepared in this embodiment 1 H NMR spectrum Fig.15 Observation Fig.15 It can be seen that the main chain segments in the polymer are AB and ABB structural chain segments, and no homopolymer chain segments of formaldehyde are generated, indicating that the product is a random copolymer containing AB and ABB chain segments.
[0113] Table 1
[0114]
[0115] 1 M n : number average molecular weight, determined by gel permeation chromatography; 2 PDI: Molecular weight distribution, determined by gel permeation chromatography.
[0116] The applicant declares that the present invention illustrates the detailed method of the present invention through the above embodiments, but the present invention is not limited to the above detailed method.
Claims
1. A polyaldehyde ester prepared by copolymerization of formaldehyde and acid anhydride, characterized in that: The general structural formula is shown in the following formulas (I) to (VI): In the formula, n1 to n6 are independently selected from integers of 0 to 1000, and m1 to m6 are independently selected from integers of 0 to 1000.
2. The polyaldehyde ester prepared by copolymerization of formaldehyde and acid anhydride according to claim 1, characterized in that: In the general structural formula, m2 to m4 are all equal to 0.
3. The polyaldehyde ester prepared by copolymerization of formaldehyde and acid anhydride according to claim 1, characterized in that: In the general structural formula, n5 to n6 are all equal to 0.
4. A method for preparing polyaldehyde ester according to any one of claims 1 to 3, characterized in that: include: The polyaldehyde ester is prepared by using formaldehyde and / or trioxymethylene and cyclic anhydride as raw materials and Lewis acid or protonic acid as catalyst through alternating copolymerization; The cyclic anhydride is selected from one or more of SA, GA, 3-MGA, 3-iBuGA, DGA, and TDGA.
5. The method for preparing polyaldehyde ester according to claim 4, wherein: The Lewis acid is selected from one or more of BF3, B(C6F5)3, InCl3, InBr3, SnCl4, AlCl3, SbCl5, PF5, CF3SO3Et, and Ph3CPF6; The protonic acid is selected from one or more of HBF4, HClO4, HN(SO2CF3)2, HN(SO2)2(CF2)3, CF3COOH, CF3SO4H, FSO4H and concentrated sulfuric acid.
6. The method for preparing polyaldehyde ester according to claim 4, wherein: The cyclic anhydride is selected from one or more of GA, 3-MGA, and 3-iBuGA; The catalyst is selected from protonic acids.
7. The method for preparing polyaldehyde ester according to claim 4, characterized in that: The cyclic anhydride is selected from DGA and / or TDGA; The catalyst is selected from protonic acids.
8. The method for preparing polyaldehyde ester according to claim 1, characterized in that: The molar ratio of formaldehyde to cyclic anhydride is 0.1 to 10:1; The molar ratio of trioxymethylene to cyclic anhydride is 0.1 to 10:3; The molar ratio of the catalyst to the cyclic anhydride is 1:10-2000; The alternating copolymerization is carried out at 80-120°C under autogenous pressure.
9. The method for preparing polyaldehyde ester according to claim 8, characterized in that: The molar ratio of formaldehyde to cyclic anhydride is 0.5 to 2.0:1; The molar ratio of trioxymethylene to cyclic anhydride is 0.5 to 2.0:3; The molar ratio of the catalyst to the cyclic anhydride is 1:20-2000.
10. The method for preparing polyaldehyde ester according to claim 9, characterized in that: The molar ratio of formaldehyde to cyclic anhydride is 1:1; The molar ratio of trioxymethylene to cyclic anhydride is 1:3; The molar ratio of the catalyst to the cyclic anhydride is 1:100-2000.
Citation Information
Patent Citations
Polyester with main chain containing acetal group and preparation method of polyester
CN113861395A
Copolymer of formaldehyde and method for manufacturing the same
GB1000673A
Method for producing polyacetal-polyesters from cyclic anhydrides and aldehydes
WO2015135948A1