Preparation method of biphenyl type low-dielectric-loss low-CTE polyimide film
The synthesis of a biphenyl-type polyimide film addresses the dielectric and thermal stability challenges by incorporating a controlled thermal process, achieving low dielectric loss and CTE suitable for 5G communication and microelectronic packaging.
Patent Information
- Application Number
- CN202411318554.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyimide materials face challenges in meeting the low dielectric loss and low CTE requirements for 5G communication and microelectronic packaging due to their high dielectric constant, dielectric loss, and hygroscopicity, necessitating improvements in thermal stability and mechanical strength.
A method involving the synthesis of a biphenyl-type diamine monomer through Suzuki coupling, followed by polymerization with dianhydride monomers to form a polyimide film, utilizing a controlled thermal imidization process to achieve low dielectric loss and low CTE.
The method results in a polyimide film with a dielectric constant of 3.01 and dielectric loss of 10.5‰, along with a CTE of 2.4ppm/K, enhancing thermal stability and reducing molecular chain irregularity.
Smart Images

Figure CN119081114A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation and application of polyimide, and relates to a method for preparing a polyimide film with low dielectric loss and low CTE. Background Art
[0002] As a high-performance engineering plastic, polyimide has attracted much attention due to its excellent thermal stability, mechanical strength, electrical insulation and other excellent properties. However, existing polyimide materials still face performance bottlenecks under specific technical challenges, such as the low dielectric performance requirements of 5G communication technology for antenna substrate materials and the high requirements of microelectronic packaging for thermal stability and mechanical strength. This paper developed a new type of polyimide material through the innovation of molecular design and synthesis path, and deeply explored the relationship between its structure and performance, providing a new theoretical direction for the design and synthesis of high-performance polymer materials.
[0003] However, with the rapid development of 5G communication, the traditional interlayer dielectric material polyimide PI needs to be modified due to its inherent high dielectric constant, high dielectric loss and high hygroscopicity, otherwise it is difficult to meet the requirements of 5G communication. PI needs to meet both low dielectric loss and low CTE. The currently disclosed PI with the lowest thermal expansion coefficient is improved by adding inorganic particles with low thermal expansion coefficient. Inorganic materials have a small thermal expansion coefficient. Adding inorganic fillers to polyimide is a common method to improve the thermal stability of polyimide. In addition, rigid non-planar structures can be added to the polyimide system. The introduction of these structures can effectively reduce the density and regularity of the PI chain, which ultimately leads to a reduction in the number of unit body active molecules, reducing the dielectric constant and the thermal expansion coefficient. Summary of the invention
[0004] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a polyimide film with low dielectric loss and high thermal stability. By increasing the amount of biphenyl, the dielectric loss of the polyimide film is reduced to only 10.5‰ and the dielectric constant is reduced to 3.01.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A method for preparing a biphenyl type low dielectric loss and low CTE polyimide film comprises the following steps:
[0006] Synthesizing a diamine monomer having a biphenyl structure, wherein the diamine monomer is one or more of the following compounds: p-aminophenylboronic acid, p-bromoaminobenzene, 14-phenyldiboronic acid, 44'-biphenyldiboronic acid;
[0007] Taking a diamine as an example, p-aminophenylboronic acid and p-bromoaminobenzene were added to a 1,4-dioxane solution at room temperature. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. Stir and reflux for 16 hours under a nitrogen atmosphere. After cooling to room temperature, the mixture was filtered, and the filter cake was repeatedly washed with water until the filtrate was almost colorless. The DMSO was recrystallized to obtain a light yellow powder.
[0008] Under room temperature conditions, diamine monomers and dianhydride monomers are polymerized in a solvent for 24 hours to undergo an amidation reaction to obtain a polyamic acid solution, wherein the dianhydride monomer is one or more of the following compounds: 6FDA, BPDA, and the solvent is N,N-dimethylacetamide (DMAc) with a purity of 99%;
[0009] The PAA solution was spread on a glass plate by using a coater at a speed of 10 mm / s to form a uniform liquid film;
[0010] The liquid film is subjected to thermal imidization reaction in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd. according to a gradient temperature increase to obtain the polyimide film, wherein the gradient temperature increase is: 80°C for 30 minutes, 120°C for 30 minutes, 160°C for 30 minutes, 200°C for 30 minutes, 250°C for 30 minutes, 300°C for 30 minutes, and 320°C for 10 minutes;
[0011] The thermally imidized film was naturally cooled, and a glass plate was immersed in a water bath at 80°C to remove the film, and then the obtained film was dried at 100°C.
[0012] Preferably, the diamine monomer is one or more of the following compounds: BZD, DPT, DMP;
[0013] Its chemical formula is:
[0014]
[0015] Preferably, the dianhydride monomer is one or more of the following compounds: 6FDA, BPDA;
[0016] Its chemical formula is:
[0017]
[0018] Preferably, the polyimide film has a dielectric constant of 3.01 to 3.61, a dielectric loss of 4.7‰ to 15.3‰, and a CTE of 2.4ppm / K to 30ppm / K.
[0019] Preferably, the solvent for polymerizing the diamine monomer and the dianhydride monomer is DMAC or DMF.
[0020] Beneficial Effects
[0021] The present invention provides a method for preparing a biphenyl type low dielectric loss low CTE polyimide film. It has the following beneficial effects: the method for preparing the biphenyl type low dielectric loss low CTE polyimide film, by adding the number of benzene rings in the monomer synthesis process, makes the arrangement of the molecular chain more regular, and improves the thermal stability of the film. The biphenyl type diamine monomer successfully synthesized by the Suzuki coupling method of the present invention reduces the dielectric constant of the polymer after polymerization, reduces the dielectric loss and reduces the CTE at the same time, and the polyimide film reaches a dielectric constant of 3.01 and a dielectric loss of 10.5‰, and the CTE reaches 2.4ppm / K. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the polymerization process of the polyimide film of the present invention. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] By those skilled in the art, the components in this case are connected in sequence. The specific connection and operation sequence should refer to the following working principle. The detailed connection means are well-known technologies in the field. The following mainly introduces the working principle and process.
[0025] See also Figure 1 The present invention provides a technical solution: a method for preparing a polyimide film with low dielectric loss and high thermal stability, comprising the following steps:
[0026] 1) Synthesize a diamine monomer having a biphenyl structure using the following compounds:
[0027]
[0028] 2) polymerizing the diamine monomer and the dianhydride monomer in a solvent for 24 hours at room temperature to produce an amidation reaction to obtain a polyamic acid solution;
[0029] The ratio of the amount of diamine monomer to the amount of dianhydride monomer added is 1:1;
[0030] The dianhydride monomer is one or more of the following two compounds:
[0031]
[0032] The diamine monomer is one or more of the following three compounds:
[0033]
[0034] 3) The polyamic acid solution was spread on a glass plate by a coating machine at a speed of 10 mm / s to form a uniform liquid film;
[0035] 4) The liquid film is subjected to thermal imidization reaction in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd. at a gradient temperature increase to obtain the polyimide film.
[0036] [Example 1]
[0037] At room temperature, 5.478g (0.04mol) of p-aminophenylboronic acid and 6.881g (0.04mol) of p-bromoaminobenzene were added to a 1,4-dioxane solution. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. The reaction mixture was stirred at 65°C and refluxed under nitrogen atmosphere for 16h. After cooling to room temperature, the filter cake was repeatedly washed with water until the filtrate was nearly colorless, and DMSO was recrystallized to obtain 8.596g of light yellow powder with a yield of 88%. Named BZD.
[0038] 4.4401g (0.0241mol) of diamine BZD and 75.7315g of solvent N, N-dimethylacetamide (DMAc) were added to a 100mL round-bottom flask and stirred for about 30 minutes. After BZD was completely dissolved, 10.7062g (0.0241mol) of 6FDA was added and mixed continuously for 24 hours at ambient temperature. Then, the resulting polyamic acid (PAA) solution was coated on a clean glass substrate, and the liquid film was subjected to a programmed temperature imidization in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd., as shown below: 80°C / 30min, 120°C / 30min, 160°C / 30min, 200°C / 30min, 250°C / 30min, 300°C / 30min, 320°C / 10min. After natural cooling, the glass plate was immersed in a water bath at 80°C to remove the film. Finally, the obtained film was dried at 100°C to obtain a high temperature resistant polyimide film with low dielectric loss. The dielectric constant was measured to be 3.23, the dielectric loss was 15.3‰, and the CTE was 30ppm / K.
[0039] [Example 2]
[0040] At room temperature, 6.630g (0.04mol) of 1,4-phenylenediboronic acid and 13.762g (0.08mol) of p-bromoaminobenzene were added to a 1,4-dioxane solution. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. The reaction mixture was stirred at 65°C and refluxed for 16h under a nitrogen atmosphere. After cooling to room temperature, the filter cake was repeatedly washed with water until the filtrate was nearly colorless, and 9.993g of light yellow powder was obtained by recrystallization from DMSO with a yield of 78%. It was named DPT.
[0041] 6.2740g (0.0241mol) of diamine DPT and 84.901g of solvent N, N-dimethylacetamide (DMAc) were added to a 100mL round-bottom flask and stirred for about 30 minutes. After DPT was completely dissolved, 10.7062g (0.0241mol) of 6FDA was added and mixed continuously at ambient temperature for 24 hours. Then, the resulting polyamic acid (PAA) solution was coated on a clean glass substrate, and the liquid film was subjected to programmed temperature imidization in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd. as follows: 80°C / 30min, 120°C / 30min, 160°C / 30min, 200°C / 30min, 250°C / 30min, 300°C / 30min, 320°C / 10min. After natural cooling, the glass plate was immersed in a water bath at 80°C to remove the film. Finally, the obtained film was dried at 100°C to obtain a high temperature resistant polyimide film with low dielectric loss. The dielectric constant was measured to be 3.08, the dielectric loss was 12.4‰, and the CTE was 24ppm / K.
[0042] [Example 3]
[0043] At room temperature, 9.6736g (0.04mol) of 4,4'-biphenyl diboronic acid and 13.762g (0.08mol) of p-bromoaminobenzene were added to a 1,4-dioxane solution. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. The reaction mixture was stirred at 65°C and refluxed under nitrogen atmosphere for 16h. After cooling to room temperature, the filter cake was repeatedly washed with water until the filtrate was almost colorless, and DMSO was recrystallized to obtain 11.408g of brown-yellow crystals with a yield of 72%. Named DMP.
[0044] 8.1080g (0.0241mol) of diamine DMP and 94.071g of solvent N, N-dimethylacetamide (DMAc) were added to a 100mL round-bottom flask and stirred for about 30 minutes. After DMP was completely dissolved, 10.7062g (0.0241mol) of 6FDA was added and mixed continuously for 24 hours at ambient temperature. Then, the resulting polyamic acid (PAA) solution was coated on a clean glass substrate, and the liquid film was subjected to a programmed temperature imidization in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd., as shown below: 80°C / 30min, 120°C / 30min, 160°C / 30min, 200°C / 30min, 250°C / 30min, 300°C / 30min, 320°C / 10min. After natural cooling, the glass plate was immersed in a water bath at 80°C to remove the film. Finally, the obtained film was dried at 100°C to obtain a high temperature resistant polyimide film with low dielectric loss. The dielectric constant was measured to be 3.01, the dielectric loss was 10.5‰, and the CTE was 2.8ppm / K.
[0045] [Example 4]
[0046] At room temperature, 5.478g (0.04mol) of p-aminophenylboronic acid and 6.881g (0.04mol) of p-bromoaminobenzene were added to a 1,4-dioxane solution. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. The reaction mixture was stirred at 65°C and refluxed under nitrogen atmosphere for 16h. After cooling to room temperature, the filter cake was repeatedly washed with water until the filtrate was nearly colorless, and DMSO was recrystallized to obtain 8.596g of light yellow powder with a yield of 88%. Named BZD.
[0047] 4.4401g (0.0241mol) of diamine BZD and 57.654g of solvent N, N-dimethylacetamide (DMAc) were added to a 100mL round-bottom flask and stirred for about 30 minutes. After BZD was completely dissolved, 7.0907g (0.0241mol) of BPDA was added and mixed continuously for 24 hours at ambient temperature. Then, the resulting polyamic acid (PAA) solution was coated on a clean glass substrate, and the liquid film was subjected to a programmed temperature imidization in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd., as shown below: 80°C / 30min, 120°C / 30min, 160°C / 30min, 200°C / 30min, 250°C / 30min, 300°C / 30min, 320°C / 10min. After natural cooling, the glass plate was immersed in a water bath at 80°C to remove the film. Finally, the obtained film was dried at 100°C to obtain a high temperature resistant polyimide film with low dielectric loss. The dielectric constant was measured to be 3.61, the dielectric loss was 8.2‰, and the CTE was 3.6ppm / K.
[0048] [Example 5]
[0049] At room temperature, 6.630g (0.04mol) of 1,4-phenylenediboronic acid and 13.762g (0.08mol) of p-bromoaminobenzene were added to a 1,4-dioxane solution. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. The reaction mixture was stirred at 65°C and refluxed for 16h under a nitrogen atmosphere. After cooling to room temperature, the filter cake was repeatedly washed with water until the filtrate was nearly colorless, and 9.993g of light yellow powder was obtained by recrystallization from DMSO with a yield of 78%. It was named DPT.
[0050] 6.2740 g (0.0241 mol) of diamine DPT and 66.8235 g of solvent N, N-dimethylacetamide (DMAc) were added to a 100 mL round-bottom flask and stirred for about 30 minutes. After DPT was completely dissolved, 7.0907 g (0.0241 mol) of BPDA was added and mixed continuously at ambient temperature for 24 hours. Then, the resulting polyamic acid (PAA) solution was coated on a clean glass substrate, and the liquid film was subjected to programmed temperature imidization in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd. as follows: 80°C / 30min, 120°C / 30min, 160°C / 30min, 200°C / 30min, 250°C / 30min, 300°C / 30min, 320°C / 10min. After natural cooling, the glass plate was immersed in a water bath at 80°C to remove the film. Finally, the obtained film was dried at 100°C to obtain a high temperature resistant polyimide film with low dielectric loss. The dielectric constant was measured to be 3.50, the dielectric loss was 5.6‰, and the CTE was 3ppm / K.
[0051] [Example 6]
[0052] At room temperature, 9.6736g (0.04mol) of 4,4'-biphenyl diboronic acid and 13.762g (0.08mol) of p-bromoaminobenzene were added to a 1,4-dioxane solution. After stirring for ten minutes, K2CO3 solution and Pd[P(C6H5)3]4 were added to the mixture, and then deoxygenated with nitrogen three times. The reaction mixture was stirred at 65°C and refluxed under nitrogen atmosphere for 16h. After cooling to room temperature, the filter cake was repeatedly washed with water until the filtrate was almost colorless, and DMSO was recrystallized to obtain 11.408g of brown-yellow crystals with a yield of 72%. Named DMP.
[0053] 8.1080g (0.0241mol) of diamine DMP and 75.994g of solvent N, N-dimethylacetamide (DMAc) were added to a 100mL round-bottom flask and stirred for about 30 minutes. After DMP was completely dissolved, 7.0907g (0.0241mol) of BPDA was added and mixed continuously for 24 hours at ambient temperature. Then, the resulting polyamic acid (PAA) solution was coated on a clean glass substrate, and the liquid film was subjected to a programmed temperature imidization in a blast drying oven of Shanghai Yiheng Scientific Instrument Co., Ltd., as shown below: 80°C / 30min, 120°C / 30min, 160°C / 30min, 200°C / 30min, 250°C / 30min, 300°C / 30min, 320°C / 10min. After natural cooling, the glass plate was immersed in a water bath at 80°C to remove the film. Finally, the obtained film was dried at 100°C to obtain a high temperature resistant polyimide film with low dielectric loss. The dielectric constant was measured to be 3.39, the dielectric loss was 4.7‰, and the CTE was 2.4ppm / K.
[0054] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions. The sentence "includes an element defined by ... does not exclude the existence of other identical elements in the process, method, article or device including the element".
[0055] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a biphenyl type low dielectric loss low CTE polyimide film, characterized in that: The following steps are involved: Synthesizing a diamine monomer having a biphenyl structure, wherein the diamine monomer is one or more of the following compounds: p-aminophenylboronic acid, p-bromoaminobenzene, 14-phenyldiboronic acid, 44'-biphenyldiboronic acid; The diamine monomer and the dianhydride monomer are polymerized in a solvent to generate an amidation reaction to obtain a polyamic acid solution, wherein the dianhydride monomer is one or more of the following compounds: 6FDA, BPDA, and the solvent is N,N-dimethylacetamide (DMAc); The polyamic acid solution is formed into a uniform liquid film by coating or casting; The liquid film is subjected to thermal imidization reaction according to a gradient temperature increase to obtain the polyimide film, wherein the gradient temperature increase is: 80°C for 30 minutes, 120°C for 30 minutes, 160°C for 30 minutes, 200°C for 30 minutes, 250°C for 30 minutes, 300°C for 30 minutes, and 320°C for 10 minutes; The thermally imidized film was naturally cooled, and a glass plate was immersed in a water bath at 80°C to remove the film, and then the obtained film was dried at 100°C.
2. The method for preparing a biphenyl type low dielectric loss low CTE polyimide film according to claim 1, characterized in that , the diamine monomer is specifically one or more of the following compounds: BZD, DPT, DMP; Its chemical formula is:
3. The method for preparing a biphenyl type low dielectric loss and low CTE polyimide film according to claim 1, characterized in that , the dianhydride monomer is one or more of the following compounds: 6FDA, BPDA; Its chemical formula is:
4. The method for preparing a biphenyl type low dielectric loss and low CTE polyimide film according to claim 1, characterized in that The polyimide film has a dielectric constant of 3.01 to 3.61, a dielectric loss of 4.7‰ to 15.3‰, and a CTE of 2.4ppm / K to 30ppm / K.
5. The method for preparing a biphenyl type low dielectric loss and low CTE polyimide film according to claim 1, characterized in that ,The solvents for polymerization of diamine monomer and dianhydride monomer are DMAC and DMF.
Citation Information
Patent Citations
Preparation method of high-temperature-resistant polyimide film with low thermal expansion coefficient
CN114380997A
Thin film for high-temperature electrostatic energy storage as well as preparation method and application of thin film
CN115093590A
Polyimide containing quaterphenyl derivative structure, diamine monomer and preparation method thereof
CN116478400A
Polyimide solution, polyimide film and flexible copper-clad plate
CN117903434A
Liquid crystal element
JP1987231937A
Cited By
The invention relates to 4, 4apos; carrying out apos; synthesis method of-diamino p-terphenyl