Large-volume alginate hydrogel and preparation method thereof
By using crosslinker microcapsule technology in sodium alginate gel, the preparation of large-volume alginate hydrogel is achieved, solving the problem of size and efficiency limitations in traditional methods, and improving the uniformity and stability of the gel , suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202411289437.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to prepare large volume sodium alginate gels, and traditional preparation methods rely on specialized equipment, are inefficient and costly, limiting their use in certain application fields.
By mixing the crosslinking agent microcapsules with sodium alginate solution, the microcapsule technology is used to achieve uniform dispersion and slow release of the crosslinking agent, which changes the traditional curing mode and crosslinking is performed under stirring and standstill conditions to prepare a large volume Alginate hydrogel.
Improves the uniformity and stability of the gel, simplifies the preparation process, improves efficiency, is suitable for a wide range of application scenarios such as biomedical and drug sustained release, and reduces dependence on special equipment.
Smart Images

Figure CN119081157A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material science, and in particular to a large-volume alginate hydrogel and a preparation method thereof. Background Art
[0002] Sodium alginate is a natural polysaccharide mainly extracted from brown algae. Due to its unique gel-forming ability, sodium alginate has been widely used in the food industry, pharmaceutical preparations, biomaterials and other fields. It reacts with multivalent metal ions (such as calcium, magnesium, zinc, etc.) in aqueous solution to form gels with different physical properties.
[0003] In the food industry, sodium alginate is widely used as a thickener, emulsifier and stabilizer due to its gel properties, stability and safety. In the pharmaceutical field, sodium alginate is mainly used in sustained-release and controlled-release preparations to improve the bioavailability and efficacy of drugs. In addition, in biomedical engineering, sodium alginate is often used in cell culture and tissue engineering due to its good biocompatibility and biodegradability.
[0004] Although sodium alginate has a wide range of applications, its traditional preparation method is mainly limited to the preparation of small-volume gels. Typically, these gels are prepared by dropping a sodium alginate solution containing an active ingredient into a cross-linker solution containing a divalent metal salt. However, this method has several limitations: (1) size limitations, which make it difficult to prepare large-volume sodium alginate gels, limiting their use in certain application areas; (2) equipment dependence, requiring specialized dropping equipment or tools, increasing production costs and complexity; (3) efficiency issues, for mass production, a large amount of dropping devices are required, resulting in a large investment, so this method is less efficient. In view of this, the present invention provides a large-volume alginate hydrogel and a method for preparing it, which will have a profound impact on related fields. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a large-volume alginate hydrogel and a preparation method thereof, with the aim of overcoming the limitations of the prior art, improving production efficiency, reducing dependence on special equipment, and expanding the application scope of sodium alginate.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] In a first aspect, a method for preparing a large-volume alginate hydrogel comprises the following steps: uniformly mixing a crosslinker microcapsule with a sodium alginate solution, crosslinking a crosslinker in the crosslinker microcapsule with sodium alginate in the sodium alginate solution to obtain an alginate hydrogel.
[0008] Based on the above technical solution, the present invention can also be improved as follows.
[0009] Furthermore, the average particle size of the crosslinking agent microcapsules is less than 100 micrometers, preferably less than 500 nanometers.
[0010] Further, the crosslinking agent microcapsules and the sodium alginate solution are uniformly mixed by stirring at 300 to 2000 rpm for 1 to 5 minutes; the crosslinking agent in the crosslinking agent microcapsules and the sodium alginate in the sodium alginate solution are crosslinked under static conditions to obtain alginate hydrogel.
[0011] Furthermore, the molar ratio of the cross-linking agent in the cross-linking agent microcapsule to the sodium alginate in the sodium alginate solution is 0.1 to 1.0.
[0012] Furthermore, the crosslinker microcapsules are mainly prepared by the following steps: dissolving the microcapsule shell material in an organic solvent to obtain a shell material solution; dispersing the crosslinker in the shell material solution to obtain a crosslinker-shell material solution dispersion system; adding a phase separation initiator to the crosslinker-shell material solution dispersion system under stirring conditions to transform the microcapsule shell material from a dissolved state to a condensed state and deposit on the particles of the crosslinker, and separating to obtain crosslinker microcapsules. Before separation, the crosslinked crosslinker-shell material solution dispersion system can be quickly transferred into a non-solvent for the shell material, and then separated to obtain crosslinker microcapsules.
[0013] Further, the microcapsule shell material includes at least one of paraffin, ethyl cellulose, acrylonitrile-butadiene-styrene copolymer (ABS), and polystyrene (PS);
[0014] The cross-linking agent includes at least one of calcium salt, magnesium salt, zinc salt, magnesium chloride, zinc chloride, magnesium nitrate, calcium chloride, etc.; the average particle size of the cross-linking agent is less than 50 microns.
[0015] The phase separation initiator includes at least one of small molecule polymers such as polydimethylsiloxane and polybutadiene;
[0016] The organic solvent includes at least one of dichloromethane, toluene and chloroform.
[0017] Furthermore, the weight ratio of the microcapsule shell material, the organic solvent, the crosslinking agent and the phase separation initiator is 1-10:100:0.05-2:100.
[0018] Furthermore, the sodium alginate solution is mainly prepared by the following steps: dissolving sodium alginate in water to obtain the sodium alginate solution, and stirring at 30° C. to 75° C. for 0.5 to 6 hours.
[0019] Furthermore, the weight ratio of the sodium alginate to the water is 0.5 to 5:100.
[0020] In a second aspect, a large-volume alginate hydrogel is provided, and the large-volume alginate hydrogel is prepared by the preparation method.
[0021] The invention disperses crosslinking agent microcapsules in a sodium alginate solution and then slowly releases the crosslinking agent to realize the crosslinking of sodium alginate to prepare hydrogel; the traditional curing mode of sodium alginate and crosslinking agent solution is changed, while the flexibility of gel volume is improved, and the preparation of large-volume alginate hydrogel is realized.
[0022] The beneficial effects of the present invention are:
[0023] (1) The present invention achieves uniform dispersion and slow release of the crosslinking agent through microencapsulation technology, solves the problem of uneven gel caused by too fast reaction between the crosslinking agent and sodium alginate, and increases the uniformity and stability of the hydrogel.
[0024] (2) The present invention improves the traditional curing mode of sodium alginate and a cross-linking agent, improves the preparation efficiency and the convenience of operation, and obtains a large-volume alginate hydrogel suitable for specific application requirements.
[0025] (3) The present invention allows the volume of the hydrogel to be flexibly adjusted according to application requirements and is suitable for a wide range of application scenarios, such as biomedicine, drug sustained release, and environmental remediation. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Photo of the large volume sodium alginate hydrogel prepared in Example 1 of the present invention;
[0027] Figure 2 Photo of the large-volume sodium alginate hydrogel prepared in Example 2 of the present invention;
[0028] Figure 3 Photo of the large-volume sodium alginate hydrogel prepared in Example 3 of the present invention;
[0029] Figure 4 Photo of the large-volume sodium alginate hydrogel prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0030] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels.
[0031] Example 1
[0032] This embodiment relates to a method for preparing a large-volume alginate hydrogel, comprising the following steps: 3 parts of paraffin wax are selected as microcapsule shell materials and dissolved in 100 parts of dichloromethane. 0.5 parts of calcium chloride powder (average particle size 38.9 microns) are dispersed in the shell material solution, and 100 parts of polydimethylsiloxane (CAS No. 9016-00-6) are slowly added as a phase separation initiator to form microcapsule powder with an average particle size of 94.1 microns.
[0033] 2 parts of sodium alginate (CAS No. 9005-38-3) were dissolved in 100 parts of water, and the mixture was stirred at 60°C for 2 hours to obtain a sodium alginate solution. The prepared crosslinker microcapsules were added to the sodium alginate solution at 1000 rpm, stirred for 5 minutes, and then transferred to a 100 mL round-bottom centrifuge tube.
[0034] After standing for 30 minutes, a large volume of alginate hydrogel with a hemispherical bottom and a total length of 6.5 cm was formed ( Figure 1 ).
[0035] Example 2
[0036] This embodiment relates to a method for preparing a large-volume alginate hydrogel, comprising the following steps: using 5 parts of ethyl cellulose (CAS No. 9004-57-3) as a microcapsule shell material, dissolving it in 100 parts of toluene. Dispersing 1 part of magnesium nitrate powder (average particle size 26.7 microns) in the shell material solution. Adding 100 parts of polybutadiene as a phase separation initiator, a microcapsule powder with an average particle size of 51.1 microns is obtained.
[0037] 1 part of sodium alginate was dissolved in 100 parts of water and stirred at 70°C for 1 hour to obtain a sodium alginate solution. The microcapsule powder was added to the sodium alginate solution at 1500 rpm, stirred for 4 minutes, and then transferred to a spherical mold. After standing for 45 minutes, a spherical large-volume alginate hydrogel with a diameter of 5.3 cm was formed ( Figure 2 ).
[0038] Example 3
[0039] This embodiment relates to a method for preparing a large-volume alginate hydrogel, comprising the following steps: 7 parts of polystyrene (CAS No. 9003-53-6) are selected as microcapsule shell materials and dissolved in 100 parts of toluene. 0.8 parts of zinc chloride powder (particle size 16.4 microns) are dispersed in the shell material solution. 100 parts of polydimethylsiloxane are slowly added to the solution as a phase separation initiator to form microcapsule powder with an average particle size of 77.5 microns.
[0040] 3 parts of sodium alginate were dissolved in 100 parts of water and stirred at 50°C for 4 hours to obtain a sodium alginate solution. The microcapsule powder was added to the sodium alginate solution at 2000 rpm, stirred for 5 minutes, and 2.5 parts were transferred to a 10 mL conical bottom centrifuge tube. After standing for 1 hour, a large volume of alginate hydrogel with a conical bottom and a total length diameter of 1.7 cm was formed ( Figure 3 ).
[0041] Example 4
[0042] This embodiment relates to a method for preparing a large-volume alginate hydrogel, comprising the following steps: using 6 parts of ABS (CAS No. 9003-56-9) as a microcapsule shell material, dissolving it in 100 parts of dichloromethane. Dispersing 1.5 parts of calcium salt powder (particle size 25.9 microns) in the shell material solution. Adding 100 parts of polybutadiene as a phase separation initiator, a microcapsule powder with an average particle size of 60.8 microns is obtained.
[0043] 4 parts of sodium alginate were dissolved in 100 parts of water and stirred at 65°C for 3 hours to obtain a sodium alginate solution. The microcapsule powder was added to the sodium alginate solution at 1800 rpm, stirred for 3 minutes, and then transferred to a watch glass with a diameter of 10 mm. After standing for 1.5 hours, a large-volume cake-shaped alginate hydrogel with a diameter of 9.3 cm was formed ( Figure 4 ).
[0044] Example 5
[0045] This embodiment relates to a method for preparing a large-volume alginate hydrogel, comprising the following steps: 8 parts of ethyl cellulose are selected as microcapsule shell materials and dissolved in 100 parts of chloroform. 0.3 parts of magnesium chloride powder (particle size 15.7 microns) are dispersed in the shell material solution. 100 parts of polydimethylsiloxane are slowly added to the solution as a phase separation initiator to obtain microcapsule powder with an average particle size of 42.1 microns.
[0046] 5 parts of sodium alginate were dissolved in 100 parts of water and stirred at 55°C for 5 hours to obtain a sodium alginate solution until it was completely dissolved. The microcapsule powder was added to the sodium alginate solution at 1500 rpm, stirred for 4 minutes, and then transferred to a 100 mL beaker.
[0047] The mixture was allowed to stand for 2 hours until the cross-linking agent ions were fully cross-linked with the sodium alginate to form a columnar large-volume alginate hydrogel with a diameter of 4.7 cm and a length of 6 cm.
[0048] In summary, the present invention can obtain a large-volume alginate hydrogel suitable for specific application requirements by adjusting the composition of the cross-linking agent microcapsule, the concentration of the sodium alginate solution, the stirring and standing time, and the final plastic mold shape and size; the present invention realizes the uniform dispersion and slow release of the cross-linking agent through microencapsulation technology, solves the problem of uneven gel caused by the too fast reaction of the cross-linking agent and sodium alginate, and increases the uniformity and stability of the hydrogel; improves the traditional curing mode of sodium alginate and the cross-linking agent, and improves the preparation efficiency and the convenience of operation.
[0049] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a large-volume alginate hydrogel, characterized in that: The method comprises the following steps: uniformly mixing crosslinking agent microcapsules with sodium alginate solution, crosslinking the crosslinking agent in the crosslinking agent microcapsules with the sodium alginate in the sodium alginate solution to obtain alginate hydrogel.
2. The method for preparing a large-volume alginate hydrogel according to claim 1, characterized in that: The average particle size of the crosslinking agent microcapsules is less than 100 microns.
3. The method for preparing a large-volume alginate hydrogel according to claim 1, characterized in that: The crosslinking agent microcapsules and the sodium alginate solution are uniformly mixed by stirring at 300 to 2000 rpm for 1 to 5 minutes; the crosslinking agent in the crosslinking agent microcapsules and the sodium alginate in the sodium alginate solution are crosslinked under static conditions to obtain alginate hydrogel.
4. The method for preparing a large-volume alginate hydrogel according to claim 1, characterized in that: The molar ratio of the cross-linking agent in the cross-linking agent microcapsule to the sodium alginate in the sodium alginate solution is 0.1 to 1.
0.
5. A method for preparing a large-volume alginate hydrogel according to any one of claims 1 to 4, characterized in that: The crosslinker microcapsules are mainly prepared by the following steps: dissolving the microcapsule shell material in an organic solvent to obtain a shell material solution; dispersing the crosslinker in the shell material solution to obtain a crosslinker-shell material solution dispersion system; adding a phase separation initiator to the crosslinker-shell material solution dispersion system under stirring conditions to transform the microcapsule shell material from a dissolved state to a condensed state and deposit it on the particles of the crosslinker, and separating to obtain crosslinker microcapsules.
6. The method for preparing a large-volume alginate hydrogel according to claim 5, characterized in that: The microcapsule shell material includes at least one of paraffin, ethyl cellulose, acrylonitrile-butadiene-styrene copolymer, and polystyrene; The cross-linking agent includes at least one of a calcium salt, a magnesium salt, and a zinc salt; The phase separation initiator includes at least one of polydimethylsiloxane and polybutadiene; The organic solvent includes at least one of dichloromethane, toluene and chloroform.
7. The method for preparing a large-volume alginate hydrogel according to claim 5, characterized in that: The weight ratio of the microcapsule shell material, the organic solvent, the crosslinking agent and the phase separation initiator is 1-10:100:0.05-2:
100.
8. A method for preparing a bulk alginate hydrogel according to any one of claims 1 to 4, characterized in that: The sodium alginate solution is mainly prepared by the following steps: dissolving sodium alginate in water to obtain the sodium alginate solution.
9. The method for preparing a large-volume alginate hydrogel according to claim 8, characterized in that: The weight ratio of the sodium alginate to the water is 0.5-5:
100.
10. A bulk alginate hydrogel, characterized in that: The large-volume alginate hydrogel is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Self-lubricating composite material, preparation method thereof and water-lubricated bearing
CN120758018A
Self-lubricating composite material, method for manufacturing same and water-lubricated bearing