NBR / PVC (nitrile butadiene rubber / polyvinyl chloride) rubber composition for high-crack-resistance static-conducting high-flame-retardant automobile fuel rubber hose and preparation method thereof

By using liquid phosphate flame retardants and environmentally friendly halogen-free phosphorus-nitrogen flame retardants in NBR/PVC rubber compositions, combining conductive carbon black and magnesium hydroxide, the process of PVC agglomeration is optimized, and the hose material is solved. The crack problems and performance balance problems at acute deformation have achieved high crack resistance, high electrostatic and flame retardant automotive fuel hose materials.

CN119081248APending Publication Date: 2024-12-06DALIAN KURASHIKI RUBBER PARTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411336301.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When the existing NBR/PVC rubber compositions are produced in fuel-type hoses, they are prone to sudden deformation of the hose and cracks at the diameter of the flush, and it is difficult to meet the requirements of conductivity, flame retardant, mechanical properties and oil resistance, especially in environmental protection. and security deficiencies.

Method used

Using the synergistic effect of liquid phosphate flame retardants, inorganic magnesium hydroxide and environmentally friendly halogen-free phosphorus-nitrogen flame retardants, combined with a small amount of conductive carbon black, the formulation and manufacturing process of NBR/PVC rubber composition is optimized, and through plasticization The two-stage kneading method reduces PVC agglomeration and improves the rubber content and mechanical properties.

Benefits of technology

It has achieved high crack resistance, static and high flame retardant automotive fuel hose materials, which meet the requirements of conductivity, flame retardancy, mechanical properties and oil resistance, avoids the crack problems of the hose at sharp bends and variable diameters, and fully meets the standards of material performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081248A_ABST
    Figure CN119081248A_ABST
Patent Text Reader

Abstract

The invention discloses a high-crack-resistance static-conductive high-flame-retardant NBR / PVC rubber composition for an automobile fuel hose and a preparation method thereof, and belongs to the technical field of rubber and plastic polymer application. The rubber composition comprises 100 parts of NBR / PVC alloy rubber, small drugs (an active agent, an anti-aging stabilizer and an internal lubricant), aniseed powder (reinforcing agent carbon black, conductive carbon black, magnesium hydroxide and an environment-friendly halogen-free phosphorus-nitrogen flame retardant), and aniseed liquid plasticizers (a phosphate flame retardant, DOTP and a vulcanization scorch retarder. During preparation of the rubber composition, plastication is added before mixing, and a high-temperature rubber discharging mode is adopted in the mixing process, so that the gathering and caking phenomenon of PVC in alloy rubber is reduced to the maximum extent, and the pipe body cracking phenomenon during diameter changing and rapid deformation of a special-shaped pipe is solved. The NBR / PVC rubber composition can bear various mutually-contained superposition properties such as flame retardance, electric conduction, oil resistance and high mechanical property, and the produced special-shaped rubber tube does not have a crack phenomenon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber and plastic polymer applications, and in particular to an NBR / PVC rubber composition for a highly crack-resistant, static-conductive and flame-retardant automobile fuel hose and a preparation method thereof. Background Art

[0002] Safety, energy saving and environmental protection are the eternal themes of the development of automobile technology. When using physical blending NBR / PVC rubber-plastic alloy glue as the main glue to produce fuel special-shaped hoses, the pipe body cracks frequently occur at the places where the hose is deformed and the diameter changes, which is a major hidden danger in production. So far, there has been no breakthrough in the industry, which directly limits the use of a large number of physical blending NBR / PVC glues in the domestic and foreign markets.

[0003] Fuel system hoses transport flammable fuels, so safety performance requirements are particularly important. To prevent static electricity accumulation, the volume resistivity of the hose material must be less than 10 6 Ω; To prevent burning, the rubber material must be flame retardant, and the hose must withstand at least 60s of flame exposure without pressure loss; to ensure safe and sealed transmission of fuel, the rubber must have excellent mechanical properties and fuel resistance: it must meet the requirements of tensile strength of more than 10MPa, elongation of more than 300%, hardness of 70±5 degrees, tear strength of more than 30KN / m, and fuel resistance volume change rate of less than 20% at 40℃×22h.

[0004] The existing conductive rubber is made by reducing the non-conductive white filler filling in the rubber formula and adding a sufficient amount of conductive carbon black, which not only ensures that the rubber composition has rubber elasticity with certain mechanical properties, but also has specific conductivity. This technology has matured and has been widely used. The existing flame retardant rubber is made by adding inorganic flame retardants (antimony trioxide, aluminum hydroxide, magnesium hydroxide, etc.) or / and organic flame retardants (bromine, nitrogen, phosphorus, etc.) to the rubber formula to absorb heat, cover, simulate chain reaction, and suffocate non-flammable gases when the polymer burns to reduce flammability. The flame retardant effects of various flame retardants have their own characteristics, but also have obvious shortcomings: inorganic flame retardants are environmentally friendly, but a large filling amount will excessively reduce the mechanical properties of the rubber composition and reduce conductivity; the most commonly used halogen flame retardant among organic flame retardants has unparalleled high efficiency, but the harm of the smoke produced to the environment and people cannot be ignored, and it is not suitable for environmental protection requirements. In addition to the above-mentioned safety properties such as conductivity and flame retardancy, the fuel hose body must also withstand severe vibration to safely and tightly transport fuel, and the rubber composition material must also have good elasticity, mechanical properties and oil resistance. Therefore, the best balance must be achieved in terms of conductivity, flame retardancy, excellent mechanical properties and oil resistance.

[0005] The existing technology cannot meet the actual requirements. For example, in terms of flame retardancy, either a small amount of bromine-based flame retardants or other environmentally unfriendly flame retardants are still used (which can ensure the mechanical properties of rubber), or a large amount of inorganic flame retardants are needed (which will inevitably increase the resistivity and reduce the physical properties of rubber), or the material meets the requirements of molded solid products such as cable pads (focusing on conductivity and flame retardancy), which are not suitable for high-performance hollow hose products. Moreover, the formulation experts have shown through years of research results on the formulation of NBR / PVC rubber compositions that single properties such as flame retardancy, conductivity, oil resistance, and high mechanical properties are easy to meet the requirements, but the various properties that restrain each other are superimposed and concentratedly carried by the NBR / PVC rubber composition, and there has been no mature use report. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a NBR / PVC rubber composition for automobile fuel hose with high crack resistance, static conductivity and high flame retardancy and a method for manufacturing the same. The rubber composition satisfies the flame retardancy requirements by selecting different types of flame retardants (an appropriate amount of liquid phosphate flame retardant and an appropriate amount of inorganic magnesium hydroxide and environmentally friendly halogen-free phosphorus nitrogen flame retardant) and producing a synergistic effect; at the same time, a small amount of conductive carbon black is added (a small amount of conductive carbon black can reduce the resistivity of the rubber due to the reduction of high-resistance white magnesium hydroxide flame retardant filler) to ensure conductivity; in terms of ensuring the mechanical properties of the rubber composition, the liquid phosphate flame retardant replaces part of the conventional plasticizer, and the corresponding reduction in the amount of low-strength white inorganic magnesium hydroxide flame retardant and low-reinforcing conductive carbon black added, on the basis of meeting the flame retardancy and conductivity of the rubber composition, the rubber content of the rubber is increased (the amount of plasticizer and non-reinforcing filler is reduced), and an appropriate amount of reinforcing carbon black ensures the higher mechanical properties of the rubber composition.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A NBR / PVC rubber composition for a highly crack-resistant, static-conductive, and flame-retardant automobile fuel hose. The raw materials for preparing the NBR / PVC rubber composition include the following components in parts by weight:

[0009]

[0010]

[0011] Furthermore, the NBR / PVC rubber-plastic alloy is a blended vulcanized rubber made of nitrile rubber (NBR) and polyvinyl chloride (PVC) by a physical blending method, and the blending weight ratio of the blending components NBR and PVC is (65-75): (25-35); the NBR / PVC rubber-plastic alloy is preferably D703L produced by Shandong Guanju Polymer Materials Co., Ltd.

[0012] Furthermore, the active agent is a mixture of zinc oxide (ZnO), magnesium oxide (MgO) and stearic acid (Sa) in a weight ratio of (3-5): (5-8): 1.

[0013] The anti-aging stabilizer is prepared by mixing an antioxidant RD, a calcium zinc stabilizer and a barium zinc stabilizer in a weight ratio of 2:(0.2-1):(0.2-1).

[0014] The internal lubricant is composed of zinc stearate and microcrystalline wax in a weight ratio of (3-6):2.

[0015] The reinforcing agent carbon black is composed of N550 and N774 in a weight ratio of (32-64): (12-26).

[0016] The vulcanization scorch retarder is prepared by mixing accelerator TT, accelerator CZ, accelerator DTDM, vulcanizing agent S-80 and scorch retarder CTP in a weight ratio of 1.5: (1.2-1.8): (0.8-1.2): (0.3-0.5): (0.3-1.0).

[0017] The method for preparing the NBR / PVC rubber composition for automobile fuel hose with high crack resistance, static conductivity and flame retardancy comprises: plasticizing the NBR / PVC rubber-plastic alloy prepared by physical blending method before mixing, and then mixing in two stages;

[0018] Physically blended NBR / PVC alloy rubber is made by mixing PVC plastic and NBR rubber in a certain proportion through mechanical equipment. Since coarse-grained PVC plastic is difficult to be completely compatible with NBR rubber (even if the PVC is pre-swelled before blending), the PVC plastic in the two phases of the alloy rubber is very easy to aggregate and agglomerate. When the rubber is vulcanized, the NBR rubber undergoes cross-linking and shrinkage, while the PVC does not participate in the reaction and phase separation occurs, especially at sharp bends and diameter changes in the hose (the thinner the rubber thickness, the more obvious the PVC aggregation). When the NBR and PVC separate, it causes macroscopic cracks in the rubber, resulting in major quality risks.

[0019] In order to overcome the problem of pipe cracks that may be caused by the easy aggregation of PVC, NBR / PVC alloy glue synthesized by NBR and PVC autoclave emulsion polymerization can be used (PVC molecules and NBR rubber molecules undergo a chain reaction and will not produce independent PVC plastic aggregation). However, since the emulsion polymerization production equipment is expensive, the manufacturing process is complicated, and there are only a few companies in the world that use emulsion polymerization to synthesize, the price of the alloy glue is high (several times the price of a large number of commonly used physical blended NBR / PVC alloy glues on the market), it is not within the scope of consideration of the present invention.

[0020] The invention aims at the NBR / PVC alloy rubber produced by physical blending method which is supplied in large quantities in the existing market, and reduces or even removes the possible PVC agglomerated particles through compulsory plasticizing processing, thereby solving the problem of frequent cracks in the production of special-shaped pipes using the NBR / PVC alloy rubber produced by physical blending method.

[0021] Specific method: Use existing rubber refining equipment to strengthen the plasticization of the physically blended NBR / PVC alloy rubber before mixing, and mechanically crush any large particles of PVC plastic that may exist to the minimum acceptable level (so that when the rubber is vulcanized, the PVC agglomerated particles will not separate from the NBR rubber after vulcanization shrinkage and cause the tube to rupture).

[0022] Considering that the minimum wall thickness of conventional special-shaped pipes at the diameter change and sharp deformation points is about 1.0-1.8mm, the PVC agglomerated particles must be controlled below 1mm (the small particle PVC agglomerated island phase is wrapped by the NBR rubber continuous sea phase). When the rubber is vulcanized, cross-linking occurs between adjacent NBR rubber molecules, and the island separation (macroscopic cracks) phenomenon will not occur.

[0023] The specific plasticating method of the present invention is:

[0024] 1. First, put the NBR / PVC rubber-plastic alloy produced by physical blending into the open mill for thin-pass treatment. The process and technical conditions are: roller distance <1mm, roller temperature 25-40℃, NBR / PVC alloy rubber passes through the roller 10 times, and is triangularly packaged;

[0025] 2. Let the thin-passed NBR / PVC alloy rubber rest naturally for 8 hours (to recover orientation fatigue) before use to complete rubber plasticization.

[0026] The plasticized NBR / PVC alloy rubber is mixed in two stages (the mixing process is divided into two stages, and the sheet is cooled and parked between the two stages) in an internal mixer to complete the manufacture of the NBR / PVC rubber composition.

[0027] In the first stage of the two-stage mixing method, 100 parts of NBR / PVC plasticized rubber weighed according to the formula are put into the internal mixer for mixing for 1.5 minutes; the weighed small medicines (active agent, anti-aging stabilizer, internal lubricant) are put into the internal mixer for mixing for 0.5 minutes; then the weighed bulk powder (reinforcing agent carbon black, conductive carbon black, inorganic flame retardant magnesium hydroxide, environmentally friendly halogen-free phosphorus nitrogen flame retardant) are put into the internal mixer, and then the weighed bulk liquid plasticizer (phosphate flame retardant, dioctyl terephthalate) is put into the internal mixer for mixing for 10 minutes, and the material is discharged at 145°C (before discharging, the material is lifted up at least once to clean the powder scattered at the feeding port), after the internal mixer is discharged, it is put into the open mixer to turn the rubber, cool and slice, and the obtained masterbatch is stored for 8 hours for standby use;

[0028] When the second stage of the two-stage mixing method is adopted, the weighed masterbatch is put into the internal mixer for preheating for 2 minutes; then the weighed vulcanization anti-scorch agent is put into the internal mixer for mixing for 2 minutes and then discharged at below 100°C; then the discharged rubber is thin-passed on the open mixer (roller distance <1mm), and after passing the roller 3 times, the roller distance is enlarged (roller distance = 10-15mm), and after wrapping the roller, the sheet is cooled and stored for 8 hours for standby use.

[0029] The advantages and beneficial effects of the present invention are as follows:

[0030] 1. The present invention optimizes the composition of the NBR / PVC rubber composition, and obtains a rubber composition material suitable for highly crack-resistant, static-conductive and highly flame-retardant automobile fuel hose through the synergistic effect of each component and an optimized manufacturing process.

[0031] 2. Before mixing the rubber material of the present invention, the NBR / PVC rubber-plastic alloy is firstly plasticized, and the large particles of PVC plastic that may exist in the rubber-plastic alloy are mechanically rolled to a particle size of less than 1 mm, so that the small particles of PVC aggregated rubber in the island phase are fully wrapped by the NBR rubber in the continuous sea phase. When the hose is vulcanized, the adjacent NBR rubber molecules are cross-linked, and the island separation (macroscopic crack) phenomenon will not occur;

[0032] 3. The first stage of the two-stage mixing method of the present invention is discharged at 145°C, which is higher than the conventional NBR / PVC rubber composition mixing discharge temperature (120-130°C). The reasons are: (a) PVC plastic is fully softened and is easier to disperse in NBR rubber; (b) the coordinated addition of calcium zinc stabilizer and barium zinc stabilizer ensures the stability of zinc ions in PVC at high temperatures; (c) in order to prevent the scorch time from being shortened due to high-temperature mixing of NBR / PVC blends, a new anti-scorch agent CTP has been pre-added in the formula.

[0033] 4. The conductivity, flame retardancy, mechanical properties and oil resistance of the NBR / PVC rubber composition material for the highly crack-resistant, static-conductive and highly flame-retardant automobile fuel hose of the present invention all meet the requirements. When used to produce special-shaped pipes, no quality problems such as cracks are found at sharp bends and diameter changes. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a photo of comparative example 2.

[0035] Figure 2 This is a photo of comparative example 3.

[0036] Figure 3 This is a photo of comparative example 1.

[0037] Figure 4 This is a photo of Example 1. DETAILED DESCRIPTION

[0038] In order to further understand the present invention, the present invention is described below in conjunction with examples, but the examples are only for further elaboration of the features and advantages of the present invention, rather than for limiting the claims of the present invention.

[0039] The following will be described in conjunction with specific examples and comparative examples. The NBR / PVC rubber-plastic alloy described in the following examples and comparative examples is D703L from Shandong Guanju Polymer Materials Co., Ltd.;

[0040] The microcrystalline wax is LSB-20; the calcium zinc stabilizer is ADK STAB RUP-173JS (RUP-173JS), and the barium zinc stabilizer is ADK STAB AC-255E (AC-255E).

[0041] The conductive carbon black is selected as model JE6900.

[0042] The phosphate flame retardant is liquid TDCPP, which can be flame-retardant through the phosphorus and chlorine elements contained in its molecules, and can also be used as a plasticizer (reducing the large-scale use of the flammable plasticizer DOTP) through its excellent compatibility with NBR / PVC rubber.

[0043] The environmentally friendly halogen-free phosphorus-nitrogen flame retardant is SFR-3D, which reacts synergistically with the inorganic flame retardant magnesium hydroxide to generate a crust during combustion, thereby terminating combustion.

[0044] The raw material formula composition of the preparation of the NBR / PVC rubber composition of each embodiment and comparative example is shown in Table 1.

[0045] Table 1 Composition of raw materials of rubber composition of examples and comparative examples (parts by weight)

[0046]

[0047] The manufacturing methods of the NBR / PVC rubber composition of the present invention for manufacturing each embodiment and comparative example are as follows:

[0048] Comparative Example 1:

[0049] The raw materials for preparing the NBR / PVC rubber composition of this comparative example are shown in Table 1, and the specific manufacturing process is as follows:

[0050] 1. Plastication of NBR / PVC rubber-plastic alloy in internal mixer: put the original rubber into internal mixer for plastication for 20 minutes (discharge at 165℃), store it for 8 hours and then use it;

[0051] 2. Use two-stage mixing method through internal mixer:

[0052] The first stage of mixing includes the following A1-A3:

[0053] A1: Take 100 parts of NBR / PVC plasticized rubber weighed according to the composition formula and put it into an internal mixer for mixing for 1.5 minutes;

[0054] A2: According to the composition formula, 11 parts of active agent, 3 parts of anti-aging stabilizer and 8 parts of internal lubricant were weighed and put into internal mixer for mixing for 0.5 minutes;

[0055] A3: According to the formula of the composition, add 76 parts of carbon black, 25 parts of conductive carbon black, 35 parts of inorganic flame retardant magnesium hydroxide, 14 parts of environmentally friendly halogen-free phosphorus-nitrogen flame retardant SFR-3D, then add 0 parts of phosphate flame retardant TDCPP and 30 parts of plasticizer DOTP, mix for 10 minutes (after 4 minutes of mixing, start the mixing once to clean the powder scattered at the feeding port), and discharge at high temperature of 145℃. After the internal mixer is discharged, put it into the open mixer to turn the rubber, cool it down, and store the masterbatch for 8 hours before use;

[0056] The second stage of mixing includes the following B1-B3:

[0057] B1: 302 parts by weight of the masterbatch obtained after the first stage of mixing was put into an internal mixer and preheated for 2 minutes;

[0058] B2: Put the vulcanization scorch retarder weighed according to the formula (TT is 1.5 parts, CZ is 1.5 parts, DTDM is 1.0 parts, S-80 is 0.4 parts, and CTP is 0.5 parts) into the internal mixer for mixing for 2 minutes and then discharge at below 100°C;

[0059] B3: Use an open mill to thin-pass the rubber obtained in step B2 (roller distance <1 mm), pass the rollers three times, enlarge the roller distance (roller distance = 10-15 mm), wrap the rollers, and cool the lower sheet for 8 hours before use.

[0060] Embodiment 1-2:

[0061] The raw materials for preparing the NBR / PVC rubber composition of this embodiment 1-2 are shown in Table 1, and the specific manufacturing process is as follows:

[0062] 1. Plastication of NBR / PVC raw rubber in open mill: Put the commercially available NBR / PVC alloy rubber produced by physical blending method (NBR / PVC rubber and plastic alloy D703L of Shandong Guanju Polymer Material Co., Ltd.) into the open mill for thin pass treatment. The process and technical conditions are: roller distance <1mm, roller temperature 25-40℃, NBR / PVC alloy rubber passes through the roller 10 times and is triangularly packaged; then the NBR / PVC alloy rubber after thin pass is naturally parked for 8 hours (to restore orientation fatigue) before use;

[0063] 2. A two-stage mixing method is adopted by an internal mixer, and the process is the same as that of Comparative Example 1.

[0064] Comparative Example 2:

[0065] The raw materials for preparing the NBR / PVC rubber composition of this comparative example are shown in Table 1, and the specific manufacturing process is as follows:

[0066] 1. The NBR / PVC alloy rubber produced by the physical blending method purchased in the market is directly mixed in the internal mixer without plasticizing;

[0067] 2. The internal mixer adopts a two-stage mixing method. Except that the discharge temperature in the first stage of mixing is 120° C., the other processes are the same as those in Example 1.

[0068] Comparative Example 3:

[0069] The raw materials for preparing the NBR / PVC rubber composition of this comparative example are shown in Table 1, and the manufacturing process is the same as that of Example 1.

[0070] The performance tests of the above embodiments and comparative examples are shown in Table 2.

[0071] Table 2 Properties of NBR / PVC rubber compositions of Examples and Comparative Examples

[0072]

[0073] From the test results, it can be seen that the mechanical properties of the comparative example 2 without adding any flame retardant and conductive carbon black are the best, but since no flame retardant is added, although the main rubber NBR / PVC contains a certain amount of Cl - ions, but rubber, carbon black, plasticizers, etc. are all flammable materials, and the flame retardancy of the rubber composition does not meet the standards. In addition, although NBR / PVC has polar groups, the addition of various fillers to the rubber composition restricts the movement of electrons after vulcanization and cross-linking of the rubber, and the conductivity of the composition does not meet the standards.

[0074] For Comparative Example 3 in which only flame retardant is added without conductive carbon black (other components are also too much or too little), a large amount of environmentally friendly halogen-free phosphorus-nitrogen flame retardant SFR-3D reacts synergistically with inorganic flame retardant magnesium hydroxide to generate crusting during combustion, and phosphorus and chlorine elements contained in the phosphate flame retardant TDCP molecules are flame retardant, so the rubber composition has a good flame retardant effect. However, the increase in the amount of inorganic filler affects the physical properties and conductivity of the rubber composition, and the tensile strength, tear strength, compression set, low-temperature brittleness, and conductivity of the rubber compound do not meet the standards;

[0075] In view of the fact that the comprehensive performance of Comparative Examples 2 and 3 cannot meet the requirements, conductive carbon black is added to Comparative Example 1 to solve the conductivity problem, and environmentally friendly halogen-free phosphorus-nitrogen flame retardant SFR-3D and inorganic flame retardant magnesium hydroxide are added to play a flame retardant role. In order to balance the mechanical properties of the rubber formula of the composition, without adding too much flammable plasticizer DOTP, except for the low-temperature brittleness that does not meet the standard, other properties just meet the standard.

[0076] In order to reduce the low-temperature brittleness of the rubber composition, Example 1 added a liquid phosphate flame retardant TDCP which has good compatibility with NBR / PVC rubber. TDCP acts as both a flame retardant and a plasticizer, which well balances the low-temperature brittleness and flame retardancy requirements of the rubber composition, and all physical properties meet the standards.

[0077] In order to further balance the comprehensive performance of the rubber composition and the material price, Example 2 reduces the high-priced SFR-3D (from 20 parts to 10 parts), increases the lower unit price inorganic flame retardant magnesium hydroxide (from 35 parts to 45 parts), and adds liquid phosphate flame retardant TDCP (from 26 parts to 38 parts) to balance the mechanical properties and flame retardancy. After testing, the comprehensive performance of the rubber composition is all up to standard and the material price is appropriate.

[0078] The appearance pictures of the rubber hoses produced by the embodiments and comparative examples using the NBR / PVC rubber composition of the present invention are as follows: Figure 1-4 .

[0079] The above is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, and improvements and modifications that conform to the principles and novel features disclosed herein and are based on the principles of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A NBR / PVC rubber composition for a highly crack-resistant, static-conductive, and flame-retardant automobile fuel hose, characterized in that: The raw materials for preparing the NBR / PVC rubber composition include the following components by weight:

2. According to claim 1, the NBR / PVC rubber composition material for automobile fuel hose with high crack resistance, static conductivity and flame retardancy is characterized by: The NBR / PVC rubber-plastic alloy rubber is a blended vulcanized rubber made from nitrile rubber (NBR) and polyvinyl chloride (PVC) by a physical blending method, and the blending weight ratio of the blending components NBR and PVC is (65-75): (25-35).

3. According to claim 1, the NBR / PVC rubber composition material for automobile fuel hose with high crack resistance, static conductivity and flame retardancy is characterized by: The active agent is prepared by mixing zinc oxide (ZnO), magnesium oxide (MgO) and stearic acid (Sa) in a weight ratio of (3-5): (5-8):

1. The anti-aging stabilizer is prepared by mixing an antioxidant RD, a calcium zinc stabilizer and a barium zinc stabilizer in a weight ratio of 2: (0.2-1): (0.2-1).

4. The NBR / PVC rubber composition material for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to claim 1, characterized in that: The internal lubricant is composed of zinc stearate and microcrystalline wax in a weight ratio of (3-6):

2.

5. The NBR / PVC rubber composition material for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to claim 1, characterized in that: The reinforcing agent carbon black is composed of N550 and N774 in a weight ratio of (32-64): (12-26).

6. The NBR / PVC rubber composition material for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to claim 1, characterized in that: The vulcanization scorch retarder is prepared by mixing accelerator TT, accelerator CZ, accelerator DTDM, vulcanizing agent S-80 and scorch retarder CTP in a weight ratio of 1.5: (1.2-1.8): (0.8-1.2): (0.3-0.5): (0.3-1.0).

7. The method for producing the NBR / PVC rubber composition for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: (1) Before mixing, the NBR / PVC rubber-plastic alloy is first plasticized; (2) The NBR / PVC alloy rubber after plasticization is mixed in a two-stage mixing process in an internal mixer to complete the manufacture of the NBR / PVC rubber composition.

8. The method for manufacturing NBR / PVC rubber for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to claim 7, characterized in that: In step (1), the plasticizing process is to put the NBR / PVC rubber-plastic alloy produced by the physical blending method into an open mill for thin-pass treatment, and the process technical conditions are: roller distance <1mm, roller temperature 25-40°C, the NBR / PVC alloy rubber is rolled 10 times and triangularly packaged; the NBR / PVC alloy rubber after the thin-pass treatment is naturally parked for 8 hours before use.

9. The method for producing the NBR / PVC rubber composition for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to claim 7, characterized in that: In step (2), when the first stage of the two-stage mixing method is adopted, 100 parts of NBR / PVC plasticized rubber weighed according to the formula are put into the internal mixer for mixing for 1.5 minutes, and then the weighed small medicines (active agent, anti-aging stabilizer, internal lubricant) are put into the internal mixer for mixing for 0.5 minutes; then the weighed bulk powder (reinforcing agent carbon black, conductive carbon black, inorganic flame retardant magnesium hydroxide, environmentally friendly halogen-free phosphorus and nitrogen flame retardant) are put into the internal mixer, and then the weighed bulk liquid plasticizer (phosphate flame retardant, dioctyl terephthalate) is put into the internal mixer, mixed for 10 minutes, and discharged at 145°C; after the internal mixer is discharged, it is put into the open mixer for turning the rubber, cooling and sheeting, and the obtained masterbatch is stored for 8 hours for standby use.

10. The method for producing the NBR / PVC rubber composition for automobile fuel hose with high crack resistance, static conductivity and flame retardancy according to claim 7, characterized in that: In step (2), when the second stage of the two-stage mixing method is adopted, the weighed masterbatch is put into an internal mixer and preheated for 2 minutes; then the weighed vulcanization anti-scorch agent is put into the internal mixer and mixed for 2 minutes and then discharged at below 100°C; then the discharged rubber is thin-passed on an open mixer (roller distance <1mm), after rolling 3 times, the roller distance is enlarged (roller distance = 10-15mm), and after rolling, the sheet is cooled and stored for 8 hours for standby use.