Novel rubber pipe mandrel rubber material and preparation method thereof
Through the formulation and preparation process of new hose mandrel rubber material, the durability and dimensional stability of existing automobile hose mandrel under high temperature conditions are solved, and multiple uses and long life under 160℃ are achieved, reducing the Production costs and environmental pollution.
Patent Information
- Application Number
- CN202411289595.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
AI Technical Summary
The existing automotive hose mandrel materials have poor durability under high temperature conditions, short service life and unstable dimensions, resulting in increased production costs and environmental pollution.
The new rubber material formula of the hose mandrel shaft includes POR elastomer, reinforcement filler, anti-aging agent, softening plasticizer, stearic acid, zinc oxide, crosslinking agent, crosslinking additive, coupling agent and graphite powder. Preparation through plasticizing, kneading and vulcanization processes improves the dimensional stability and durability of the material.
Under high temperature conditions of 160°C, the new material exhibits small size changes and high stability, and can be used multiple times without scrapping, which extends the service life, reduces production costs and reduces environmental pollution.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber composite materials, and in particular relates to a novel hose core shaft rubber material and a preparation method thereof. Background Art
[0002] In recent years, due to the continuous expansion of automobile production, the demand for automotive rubber parts has soared. The use of automotive oil-resistant hoses, air conditioning hoses, brake hoses, and radiator hoses has also increased significantly. In addition to various hoses used in the repair of new and old cars, the domestic demand for various hose rubber materials has reached tens of millions of tons each year. The production of hoses requires the use of mandrels, which has led to a sharp increase in the use of hose mandrel rubber materials, reaching more than one million tons.
[0003] At present, the traditional materials used for domestic automotive hose mandrels are mainly nitrile rubber, nylon, etc. Although nitrile rubber has excellent physical properties, its heat resistance can only reach 120℃. The prepared hose mandrel has poor durability. After repeated use in a 160℃ thermal cycle vulcanization tank, it will age and cause the mechanical strength to decrease and become unusable. The service life is short (repeated use 2 to 4 times). Although the traditional best nylon mandrel has good heat resistance, it has poor flex resistance. After repeated use, it will stretch or shrink, resulting in unstable caliber size and scrap (repeated use 3 to 5 times). As a consumable material, the hose mandrel must not only have the flexibility to be easy to wind and the heat resistance to withstand high temperatures during vulcanization, as well as the dimensional stability under harsh thermal cycles and the durability of repeated use. Due to the poor durability and few repeated uses of traditional mandrel rubber materials, the production cost increases, the scrapped hose mandrel is difficult to handle, and the environmental pollution is large.
[0004] Therefore, it is necessary to develop a rubber material for the hose mandrel with good dimensional stability, excellent durability, and long service life (repeated use for more than dozens of times), which has good economic benefits. Summary of the invention
[0005] The purpose of the present invention is to provide a new type of hose mandrel rubber material and a preparation method thereof. The present invention is derived from the actual production needs of customers to solve the problems of poor dimensional stability, insufficient durability, short service life and few repeated uses of existing mandrel rubber materials.
[0006] A novel hose core shaft rubber material comprises the following raw materials, measured by weight: 100 parts of POR elastomer, 120-160 parts of reinforcing filler, 2-4 parts of antioxidant, 60-100 parts of softening plasticizer, 1-1.5 parts of stearic acid, 5-10 parts of zinc oxide, 3-5 parts of crosslinking agent, 2-4 parts of crosslinking aid, 3-5 parts of coupling agent, 3-6 parts of process aid and 5-10 parts of graphite powder.
[0007] Preferably, the softening plasticizer is at least two of hydrocarbon compounds with Mn=300-600, liquid EPDM, and high molecular weight paraffin oil.
[0008] Preferably, the process aid consists of liquid paraffin and paste polyethylene wax, wherein the paste polyethylene wax accounts for at least 2 parts.
[0009] Preferably, the crosslinking agent is one or two of dicumyl peroxide, di-tert-butyl peroxycumene, and 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane.
[0010] Preferably, the crosslinking aid is any one or two of N,N'-m-phenylene bismaleimide, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.
[0011] Preferably, the reinforcing filler is any one or more of carbon black, light calcium carbonate, and calcined clay; the antioxidant is any one of antioxidant MBZ, antioxidant MB, antioxidant 445, antioxidant NBC, and antioxidant DDA.
[0012] Preferably, the coupling agent is composed of a silane coupling agent and any one of a titanate coupling agent and an aluminate coupling agent, wherein the silane coupling agent is at least 2 parts.
[0013] A method for preparing a novel hose core shaft rubber material comprises the following steps: (1) Plasticizing: POR elastomer is refining in an open mill until the Mooney viscosity ML1+4 at 125°C is below 60; (2) Mixing: Add the plasticized POR elastomer, reinforcing filler, coupling agent, softening plasticizer, graphite powder and process additives into the kneader, control the speed at 60-100r / min for the first mixing for 3min, then add antioxidant, stearic acid, zinc oxide, softening plasticizer, crosslinking agent and crosslinking aid, keep the mixing temperature at 100-120℃ for the second mixing for 6-10min, discharge the material, put the cold material on the plate, stop for 24h and then heat-refined. After the rubber is hot-refined and rolled, adjust the roller distance to 0.1mm, pass it through 3 times, make 3 triangle bags, put it on the plate and stop for 6h; (3) Vulcanization: The mixed rubber obtained in step (2) is re-mixed and vulcanized at 160°C and 12-15 MPa for 30 min.
[0014] Preferably, the amount of softening plasticizer added in the first mixing in step (2) is 50% of the total softening plasticizer.
[0015] Advantages of the present invention: Compared with the existing traditional nitrile rubber mandrel and nylon mandrel, the mandrel made of the novel rubber material for the hose mandrel of the present invention has the advantages of small size change, high stability and almost unchanged hose diameter after repeated use in a 160°C high-temperature vulcanization tank for a long time. DETAILED DESCRIPTION
[0016] Example 1 A new type of hose mandrel rubber material, including the following raw materials by weight: 100 parts of POR elastomer, 130 parts of reinforcing filler, 3 parts of antioxidant, 80 parts of softening plasticizer, 1.5 parts of stearic acid, 10 parts of zinc oxide, 3 parts of crosslinking agent, 4 parts of crosslinking aid, 5 parts of coupling agent, 6 parts of process aid, and 8 parts of graphite powder; The reinforcing filler is carbon black; The antioxidant is antioxidant NBC; The softening plasticizer is a hydrocarbon compound with Mn=300-600 and a high molecular weight paraffin oil; The cross-linking agent is dicumyl peroxide; The cross-linking aid is N, N'-m-phenylene bismaleimide; The coupling agent is composed of a silane coupling agent and an aluminate coupling agent, wherein the silane coupling agent is 2 parts; The process aids are 3 parts each of liquid paraffin and paste polyethylene wax; A method for preparing a novel hose core shaft rubber material comprises the following steps: (1) Plasticizing: POR elastomer is refining in an open mill until the Mooney viscosity ML1+4 at 125°C is below 60; (2) Mixing: Add the plasticized POR elastomer, reinforcing filler, coupling agent, 50% softening plasticizer, graphite powder and process additives into the kneader, control the speed at 60r / min for the first mixing for 3min, then add antioxidant, stearic acid, zinc oxide, 50% softening plasticizer, crosslinking agent and crosslinking aid, keep the mixing temperature at 120℃ for the second mixing for 6min, discharge the material, put the cold material down, stop for 24h and then heat-refined, after the rubber is hot-refined and rolled, adjust the roller distance to 0.1mm, pass through 3 times, make 3 triangle bags, put the material down and stop for 6h; (3) Vulcanization: The rubber mixture obtained in step (2) is re-mixed and vulcanized at 160°C and 12-15 MPa for 30 min.
[0017] Example 2 A new type of hose mandrel rubber material, including the following raw materials by weight: 100 parts of POR elastomer, 120 parts of reinforcing filler, 2 parts of antioxidant, 60 parts of softening plasticizer, 1 part of stearic acid, 5 parts of zinc oxide, 4 parts of cross-linking agent, 3 parts of cross-linking aid, 4 parts of coupling agent, 5 parts of process aid, and 5 parts of graphite powder; The reinforcing filler is carbon black and calcined clay; The antioxidant is antioxidant DDA; The softening plasticizer is a hydrocarbon compound with Mn=300-600 and liquid EPDM; The cross-linking agent is di-tert-butyl peroxyisopropylbenzene; The cross-linking aid is trimethylolpropane trimethacrylate; The coupling agent is composed of a silane coupling agent and a titanate coupling agent, wherein the silane coupling agent is 2 parts; The process aids are liquid paraffin and paste polyethylene wax, wherein the paste polyethylene wax is 3 parts; A method for preparing a novel hose core shaft rubber material comprises the following steps: (1) Plasticizing: POR elastomer is refining in an open mill until the Mooney viscosity ML1+4 at 125°C is below 60; (2) Mixing: Add the plasticized POR elastomer, reinforcing filler, coupling agent, 50% softening plasticizer, graphite powder and process additives into the kneader, control the speed at 100r / min for the first mixing for 3min, then add antioxidant, stearic acid, zinc oxide, 50% softening plasticizer, crosslinking agent and crosslinking aid, keep the mixing temperature at 100℃ for the second mixing for 10min, discharge the material, put the cold material on the plate, park it for 24h and then heat-refined, after the rubber is hot-refined and rolled, adjust the roller distance to 0.1mm, pass it through 3 times, make 3 triangle bags, put it on the plate and park it for 6h; (3) Vulcanization: The rubber mixture obtained in step (2) is re-mixed and vulcanized at 160°C and 12-15 MPa for 30 min.
[0018] Example 3 A new type of hose mandrel rubber material, including the following raw materials by weight: 100 parts of POR elastomer, 160 parts of reinforcing filler, 4 parts of antioxidant, 100 parts of softening plasticizer, 1 part of stearic acid, 5 parts of zinc oxide, 5 parts of crosslinking agent, 2 parts of crosslinking aid, 3 parts of coupling agent, 3 parts of process aid, and 10 parts of graphite powder; The reinforcing filler is carbon black and light calcium carbonate; The antioxidant is antioxidant 445; The softening plasticizer is high molecular weight paraffin oil and liquid EPDM; The cross-linking agent is 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane; The cross-linking aid is trimethylolpropane triacrylate; The coupling agent is composed of a silane coupling agent and an aluminate coupling agent, wherein the silane coupling agent is 2 parts; The process aids are liquid paraffin and paste polyethylene wax, wherein the paste polyethylene wax is 2 parts; A method for preparing a novel hose core shaft rubber material comprises the following steps: (1) Plasticizing: POR elastomer is refining in an open mill until the Mooney viscosity ML1+4 at 125°C is below 60; (2) Mixing: Add the plasticized POR elastomer, reinforcing filler, coupling agent, 50% softening plasticizer, graphite powder and process additives into the kneader, control the speed at 80r / min for the first mixing for 3min, then add antioxidant, stearic acid, zinc oxide, 50% softening plasticizer, crosslinking agent and crosslinking aid, keep the mixing temperature at 110℃ for the second mixing for 8min, discharge the material, put the cold material down, stop for 24h and then heat-refined, after the rubber is hot-refined and rolled, adjust the roller distance to 0.1mm, pass through 3 times, make 3 triangle bags, put the material down and stop for 6h; (3) Vulcanization: The rubber mixture obtained in step (2) is re-mixed and vulcanized at 160°C and 12-15 MPa for 30 min.
[0019] Example 4 A new type of hose mandrel rubber material, including the following raw materials by weight: 100 parts of POR elastomer, 130 parts of reinforcing filler, 3 parts of antioxidant, 80 parts of softening plasticizer, 1 part of stearic acid, 5 parts of zinc oxide, 4 parts of cross-linking agent, 4 parts of cross-linking aid, 4 parts of coupling agent, 5 parts of process aid, and 8 parts of graphite powder; The reinforcing filler is light calcium carbonate and calcined clay; The antioxidant is antioxidant MBZ; The softening plasticizer is high molecular weight paraffin oil and liquid EPDM; The cross-linking agent is dicumyl peroxide and di-tert-butyl peroxycumene; The crosslinking aid is trimethylolpropane triacrylate and trimethylolpropane trimethacrylate; The coupling agent is composed of a silane coupling agent and an aluminate coupling agent, wherein the silane coupling agent is 2 parts; The process aids are liquid paraffin and paste polyethylene wax, wherein the paste polyethylene wax is 3 parts; A method for preparing a novel hose core shaft rubber material comprises the following steps: (1) Plasticizing: POR elastomer is refining in an open mill until the Mooney viscosity ML1+4 at 125°C is below 60; (2) Mixing: Add the plasticized POR elastomer, reinforcing filler, coupling agent, 50% softening plasticizer, graphite powder and process additives into the kneader, control the speed at 90r / min for the first mixing for 3min, then add antioxidant, stearic acid, zinc oxide, 50% softening plasticizer, crosslinking agent and crosslinking aid, keep the mixing temperature at 110℃ for the second mixing for 8min, discharge the material, put the cold material down, stop for 24h and then heat-refined, after the rubber is hot-refined and rolled, adjust the roller distance to 0.1mm, pass through 3 times, make 3 triangle bags, put the material down and stop for 6h; (3) Vulcanization: The rubber mixture obtained in step (2) is re-mixed and vulcanized at 160°C and 12-15 MPa for 30 min.
[0020] Example 5 A new type of hose mandrel rubber material, including the following raw materials by weight: 100 parts of POR elastomer, 150 parts of reinforcing filler, 4 parts of antioxidant, 90 parts of softening plasticizer, 1 part of stearic acid, 5 parts of zinc oxide, 4 parts of cross-linking agent, 3 parts of cross-linking aid, 4 parts of coupling agent, 5 parts of process aid, and 8 parts of graphite powder; The antioxidant is antioxidant DDA; The rest is the same as Example 4.
[0021] Comparative Example 1 The nitrile mandrel rubber compound formula was selected for comparison, specifically: 100 parts of nitrile 26 rubber, 100 parts of natural gas semi-reinforced carbon black, 50 parts of light calcium carbonate, 3 parts of antioxidant RD, 60 parts of DOP, 1.5 parts of stearic acid, 5 parts of zinc oxide, 7 parts of cross-linking agent and cross-linking aid, 3 parts of silane coupling agent, 4 parts of process aid, and 8 parts of DCP / S / DTDM in total.
[0022] Performance testing: The testing methods for basic mechanical physical properties (such as hardness, tensile strength, elongation at break, etc.) are carried out in accordance with national standards; Durability test: Wrap the vulcanized 2mm test piece with an unvulcanized 2mm film tightly against its surface, put it in a 160℃ oven for 60 minutes, then take it out, peel off the outer wrapping film, visually test the appearance changes of the test piece, and measure the size and basic physical properties of the test piece. This operation is repeated 12 times with the same test piece, and the test is carried out at the 1st, 4th, 8th, and 12th times; Dimensional stability test: shrinkage determination of test pieces; Note: H represents Shore hardness, T represents tensile strength, E represents elongation at break, L represents shrinkage, △H, △T, △E, △L all represent their change rate (%).
[0023] From the data in the table, it can be seen that the hardness of the rubber material of the hose mandrel of the present invention has a small change after multiple durability tests. After the 12th test, the hardness of Examples 1 to 5 varies between 0 and 4, which indicates that the material maintains a relatively stable hardness during use. The tensile strength decreases by 5.8% at most after the 12th test (Example 4), and the decrease in other examples is small, ranging from -3.6% to -5.8%. The relatively small change in tensile strength indicates that the material still maintains strong tensile properties after multiple tests; The elongation of the embodiment of the present invention decreases relatively little in multiple tests, and the decrease after the 12th test is between -12.1% and -18.9%, indicating that the material still maintains a high ductility after multiple high-temperature aging, and can adapt to a certain degree of deformation without breaking. These properties have a positive impact on the reliability of rubber materials under complex working conditions. The shrinkage rates of Examples 1 to 5 of the present invention hardly change significantly. During the entire test process, the shrinkage rate changes within a very small range (up to 1.6%). This dimensional stability means that the material will not show significant deformation or shrinkage after repeated use or aging, thereby ensuring the structural stability and service life of the material.
Claims
1. A new type of hose mandrel rubber material, characterized in that: The raw materials are as follows, in parts by weight: 100 parts of POR elastomer, 120-160 parts of reinforcing filler, 2-4 parts of antioxidant, 60-100 parts of softening plasticizer, 1-1.5 parts of stearic acid, 5-10 parts of zinc oxide, 3-5 parts of crosslinking agent, 2-4 parts of crosslinking aid, 3-5 parts of coupling agent, 3-6 parts of process aid and 5-10 parts of graphite powder.
2. The new hose core shaft rubber material according to claim 1 is characterized in that: The softening plasticizer is at least two of hydrocarbon compounds with Mn=300-600, liquid EPDM, and high molecular weight paraffin oil.
3. The new hose core shaft rubber material according to claim 1 is characterized in that: The process aid is composed of liquid paraffin and paste polyethylene wax, wherein the paste polyethylene wax accounts for at least 2 parts.
4. The new hose core shaft rubber material according to claim 1 is characterized in that: The cross-linking agent is one or two of dicumyl peroxide, di-tert-butyl peroxycumene, and 2,5-dimethyl-2,5-bis(tert-butyl peroxide)hexane.
5. The new hose core shaft rubber material according to claim 1 is characterized in that: The cross-linking auxiliary agent is any one or two of N,N'-m-phenylene bismaleimide, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.
6. The novel hose core shaft rubber material according to claim 1 is characterized in that: The reinforcing filler is any one or more of carbon black, light calcium carbonate, and calcined clay; the antioxidant is any one of antioxidant MBZ, antioxidant MB, antioxidant 445, antioxidant NBC, and antioxidant DDA.
7. The novel hose core shaft rubber material according to claim 1 is characterized in that: The coupling agent is composed of a silane coupling agent and any one of a titanate coupling agent and an aluminate coupling agent, wherein the silane coupling agent is at least 2 parts.
8. A method for preparing the novel hose core shaft rubber material according to claims 1-7, characterized in that: The following steps are involved: (1) Plasticizing: POR elastomer is refining in an open mill until the Mooney viscosity ML1+4 at 125°C is below 60; (2) Mixing: Add the plasticized POR elastomer, reinforcing filler, coupling agent, softening plasticizer, graphite powder and process additives into the kneader, control the speed at 60-100r / min for the first mixing for 3min, then add antioxidant, stearic acid, zinc oxide, softening plasticizer, crosslinking agent and crosslinking aid, keep the mixing temperature at 100-120℃ for the second mixing for 6-10min, discharge the material, put the cold material on the plate, stop for 24h and then heat-refined. After the rubber is hot-refined and rolled, adjust the roller distance to 0.1mm, pass it through 3 times, make 3 triangle bags, put it on the plate and stop for 6h; (3) Vulcanization: The mixed rubber obtained in step (2) is re-mixed and vulcanized at 160°C and 12-15 MPa for 30 min.
9. The method for preparing the novel hose core shaft rubber material according to claim 8, characterized in that: The amount of softening plasticizer added in the first mixing in step (2) is 50% of the total softening plasticizer.