Polypropylene material as well as preparation method and application thereof

Through the modified magnesium sulfate whiskers and polypropylene compounding technology, the light transmittance and mechanical properties of bumper materials in new energy vehicles are improved, and the problem that traditional materials are difficult to take into account both light transmittance and mechanical properties is solved, and high light transmittance is achieved Improve the comprehensive performance of rate, toughness and rigidity.

CN119081284AActive Publication Date: 2024-12-06WANHUA CHEMICAL (NINGBO) CO LTD

Patent Information

Application Number
CN202411247291.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-12-06
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Existing polypropylene materials are difficult to take into account high light transmittance and mechanical properties, and cannot meet the multifunctional needs of new energy vehicles based on safety performance.

Method used

Modified magnesium sulfate whiskers are modified by dispersant, surfactant and γ-aminopropyltriethoxysilane, combined with high rigid homopolypropylene and random copolymer polypropylene , and add transparent nucleating agents and antioxidants to improve the dispersion and compatibility of the material and enhance its light transmittance and mechanical properties.

Benefits of technology

The comprehensive performance of high light transmittance, toughness and rigidity of polypropylene materials is improved, and the thermal stability and heat resistance of the material are improved, solving the problem that it is difficult to take into account both the mechanical properties and light transmittance properties of traditional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005031148780000101
    Figure BDA0005031148780000101
  • Figure BDA0005031148780000111
    Figure BDA0005031148780000111
  • Figure BDA0005031148780000121
    Figure BDA0005031148780000121
Patent Text Reader

Abstract

The invention discloses a polypropylene material as well as a preparation method and application thereof, belongs to the technical field of high polymer material modification, and solves the problem that mechanical properties and high light transmittance of a polypropylene material in the prior art are difficult to consider at the same time. The polypropylene material comprises the following raw materials in parts by weight: 40-90 parts of polypropylene, 0.5-5 parts of maleic anhydride grafted polypropylene, 5-15 parts of modified magnesium sulfate whiskers, 0.2-1.0 part of a transparent nucleating agent, 5-15 parts of a toughening agent and 0.2-0.8 part of an antioxidant, the modified magnesium sulfate whisker is magnesium sulfate whisker modified by a dispersing agent, a surfactant and gamma-aminopropyltriethoxysilane. The polypropylene material has high light transmittance and mechanical properties at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material modification, and in particular relates to a polypropylene material and a preparation method and application thereof. Background Art

[0002] With the rapid development of the automobile industry in recent years, the proportion of new energy vehicles has become higher and higher. Compared with traditional oil vehicles, new energy vehicles have undergone major changes in the power system. Intelligence and technology have become a major symbol that distinguishes new energy vehicles from traditional vehicles. Traditional automobile bumper materials are mainly used as energy-absorbing and protective materials when the car is hit to improve the safety factor of the car. The development of new energy vehicles is not limited to this. While meeting the protective function, it is necessary to be able to give the material a new function. For example, on the basis of being able to meet the safety performance, the material has a certain light transmittance, a unique pattern or LOGO can be designed on it, and a backlight component can be placed behind it, thus presenting a cool sense of intelligence and technology.

[0003] Existing bumper materials improve their mechanical properties by adding whiskers into the polypropylene matrix, but this will result in poor light transmittance of the material. If whiskers are not added, the mechanical properties will be poor and it will be difficult to provide protection. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the problem in the prior art that it is difficult to balance the mechanical properties and high light transmittance of polypropylene materials, thereby providing a polypropylene material and a preparation method and application thereof.

[0005] To this end, the present invention provides the following technical solutions.

[0006] In a first aspect, the present invention provides a polypropylene material, wherein the raw materials include, by weight:

[0007] 40-90 parts of polypropylene, 0.5-5 parts of maleic anhydride grafted polypropylene, 5-15 parts of modified magnesium sulfate whiskers, 0.2-1.0 parts of transparent nucleating agent, 5-15 parts of toughening agent, 0.2-0.8 parts of antioxidant;

[0008] The modified magnesium sulfate whisker is magnesium sulfate whisker modified by a dispersant, a surfactant and gamma-aminopropyltriethoxysilane.

[0009] Furthermore, the preparation method of the modified magnesium sulfate whisker comprises:

[0010] S1: Mixing magnesium sulfate whiskers, water and a dispersant, adjusting the pH to 4-6, reacting, and then separating the solid from the liquid, washing and drying the solid to obtain pre-dispersed magnesium sulfate whiskers;

[0011] S2: pre-dispersed magnesium sulfate whiskers, surfactants, γ-aminopropyltriethoxysilane and solvents are mixed, reacted, and then solid-liquid separation is performed, and the solid is washed and dried to obtain modified magnesium sulfate whiskers.

[0012] Furthermore, the preparation method of the modified magnesium sulfate whisker satisfies at least one of the following conditions:

[0013] (1) In S2, the mass ratio of the pre-dispersed magnesium sulfate whiskers, the surfactant and γ-aminopropyltriethoxysilane is (100-300): (0.1-0.5): (5-25), preferably (100-200): (0.1-0.3): (15-25);

[0014] (2) The reaction conditions of S2 are: reaction at a temperature of 60 to 80°C for 12 to 24 hours;

[0015] (3) The reaction atmosphere of S2 is nitrogen;

[0016] (4) The step of mixing the pre-dispersed magnesium sulfate whiskers, surfactant, γ-aminopropyltriethoxysilane and solvent in S2 comprises: firstly adding the pre-dispersed magnesium sulfate whiskers into the solvent for ultrasonic dispersion, and then adding the surfactant and γ-aminopropyltriethoxysilane; the ultrasonic dispersion can further disperse the pre-dispersed magnesium sulfate whiskers, so that the substances added later can have a more complete contact reaction;

[0017] Optionally, the ultrasonic dispersion time is 0.25 to 0.75 h;

[0018] Optionally, the solvent is anhydrous ethanol.

[0019] Furthermore, the preparation method of the modified magnesium sulfate whisker satisfies at least one of the following conditions:

[0020] (1) In S1, the step of mixing magnesium sulfate whiskers, water and a dispersant comprises: adding magnesium sulfate whiskers to water for ultrasonic dispersion, and then adding a dispersant;

[0021] Optionally, the ultrasonic dispersion time is 0.5 to 1.0 h;

[0022] (2) The reaction conditions in S1 are 50-70°C for 1-3h;

[0023] (3) In S1, the mass of the dispersant is 5.0-10.0% of the mass of the magnesium sulfate whiskers;

[0024] (4) In S1, the aspect ratio of the magnesium sulfate whisker is greater than 30, and preferably the aspect ratio is 35-100.

[0025] Furthermore, at least one of the following conditions is met:

[0026] (1) The dispersant is at least one selected from tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide;

[0027] (2) The surfactant is at least one selected from sodium dodecyl sulfonate (SDS), sodium dodecyl sulfate and sodium stearate.

[0028] Furthermore, the melt flow rate of the maleic anhydride grafted polypropylene is greater than 15 g / 10 min, and the maleic anhydride grafting rate is 0.5% to 2.0%.

[0029] Further, the polypropylene is selected from one or more of homopolymer polypropylene and copolymer polypropylene;

[0030] Optionally, the polypropylene is compounded by high rigidity homopolymer polypropylene and random copolymer polypropylene in a mass ratio of (30-50):(20-40);

[0031] The high rigidity homopolymer polypropylene resin has a melt flow rate of 5 to 100 g / 10 min and a bending modulus of >1800 MPa;

[0032] The random copolymer polypropylene is a polymer obtained by random copolymerization of propylene and ethylene, and has a melt flow rate of 1 to 10 g / 10 min.

[0033] Furthermore, at least one of the following conditions is met:

[0034] (1) The transparent nucleating agent is selected from one or more of carboxylic acid metal salt nucleating agents, sorbitol nucleating agents, and aromatic phosphate nucleating agents;

[0035] (2) The toughening agent is selected from one or more of vinyl-polydiene-styrene block copolymer, styrene-ethylene-butadiene-styrene copolymer, ethylene-octene copolymer, and ethylene-butene copolymer;

[0036] (3) The antioxidant is selected from one or more of hindered phenol antioxidants, hindered amine antioxidants, phosphite antioxidants, thiodipropionate antioxidants, and thiol antioxidants, preferably hindered phenol antioxidants and phosphite antioxidants;

[0037] Preferably, the mass ratio of hindered phenol antioxidant to phosphite antioxidant is (0.1-0.3):(0.1-0.3).

[0038] In a second aspect, the present invention provides a method for preparing a polypropylene material, characterized in that it comprises the following steps:

[0039] S1: Add various raw material components into a high-speed mixer for mixing according to the formula;

[0040] S2: adding the premixed materials in step S1 into a twin-screw extruder, melt blending, extruding and granulating to obtain the polypropylene material;

[0041] Optionally, the mixing condition of the high-speed mixer is 600 to 1000 r / min for 2 to 5 min;

[0042] Optionally, the temperature of the twin-screw extruder is between 180° C. and 220° C., and the screw speed is between 500 and 900 r / min.

[0043] In a third aspect, the present invention provides a bumper, comprising the above-mentioned polypropylene material or the polypropylene material prepared according to the above-mentioned method.

[0044] The technical solution of the present invention has the following advantages:

[0045] 1. The raw materials of the polypropylene material of the present invention include, by weight: 40 to 90 parts of polypropylene, 0.5 to 5 parts of maleic anhydride grafted polypropylene, 5 to 15 parts of modified magnesium sulfate whiskers, 0.2 to 1.0 parts of transparent nucleating agent, 5 to 15 parts of toughening agent, and 0.2 to 0.8 parts of antioxidant; the modified magnesium sulfate whiskers are magnesium sulfate whiskers modified by a dispersant, a surfactant and γ-aminopropyltriethoxysilane.

[0046] The invention adopts a dispersant, a surfactant and gamma-aminopropyl triethoxysilane to modify the magnesium sulfate whisker, wherein the dispersant can be adsorbed on the surface of the magnesium sulfate whisker, and the dispersibility of the magnesium sulfate whisker is greatly improved under the action of electrostatic repulsion, and agglomeration is avoided, thereby promoting the surfactant and gamma-aminopropyl triethoxysilane to perform amino modification on the magnesium sulfate whisker, and the amino modification can cause the anhydride group on the maleic anhydride grafted polypropylene in the formula to react with -NH2 on the surface of the magnesium sulfate whisker to generate an interface compatibilization reaction, so that the dispersant and compatibility of the magnesium sulfate whisker in the matrix are further improved, so that the polypropylene material has both high light transmittance and mechanical properties.

[0047] The modified magnesium sulfate whiskers have a needle-like structure, which plays a supporting role in the material, restricting the movement of polymer molecules during the heating process, thereby improving the thermal stability of the material.

[0048] 2. Polypropylene is compounded by high rigidity homopolymer polypropylene and random copolymer polypropylene in a mass ratio of (30-50):(20-40);

[0049] High-rigidity PP has a higher modulus, and random PP has higher toughness. The two are compounded, utilizing the advantages of high rigidity and high heat resistance of high-rigidity homopolymer polypropylene to improve the heat resistance temperature and rigidity of the material. Combined with transparent nucleating agents to reduce the grain size of spherulites, the transmittance is further increased, making the polypropylene material have excellent comprehensive properties such as transmittance, toughness and rigidity.

[0050] 3. The mass ratio of the pre-dispersed magnesium sulfate whiskers, surfactant and γ-aminopropyltriethoxysilane is (100-200): (0.1-0.3): (15-25). Within this limited range, the dispersion of the modified magnesium sulfate whiskers in the material and the compatibility with the matrix can be optimized, thereby promoting the overall toughness and transmittance of the polypropylene material to reach the best. DETAILED DESCRIPTION

[0051] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0052] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0053] The main test methods involved in the following embodiments of the present invention are as follows:

[0054] <1> Mechanical properties test:

[0055] Bending performance: Use ZWICK's Z010 universal testing machine to test in accordance with ISO 178:2019 standard;

[0056] Izod notched impact: The test was conducted using a ZWICK HIT25P impact tester in accordance with ISO 180:2019.

[0057] <2> Light transmittance test: Use X-Rite CI7860 desktop colorimeter to test the 2mm and 3mm color plates of injection molding in transmission mode according to ASTM D1003-2013 standard;

[0058] <3> Load heat deformation temperature test: using INSTRON HV6M thermal analyzer, under 0.45MPa pressure, in accordance with ISO 75-2:2013 standard;

[0059] <4> Shrinkage test: The extruded particles were injected into 350*70*3mm plates using a single-screw injection molding machine, conditioned at constant temperature and humidity for 48 hours, and the dimensional changes were detected using a test fixture;

[0060] The main raw material information in the following examples of the present invention is as follows:

[0061] (1) PP-6012: high rigidity homopolymer polypropylene, melt flow rate 10g / 10min (230℃, 2.16kg), Tianjin Petrochemical;

[0062] (2) PP-M60T: high rigidity homopolymer polypropylene, melt flow rate 60g / 10min (230℃, 2.16kg), Zhenhai Refining and Chemical;

[0063] (3) QCT02N: random copolymer polypropylene, melt flow rate 5 g / 10 min (230 °C, 2.16 kg), Ningqilu Petrochemical;

[0064] (4) 5012XT: random copolymer polypropylene, melt flow rate 3 g / 10 min (230 °C, 2.16 kg), Ningbo Formosa Plastics;

[0065] (5) WS-152: magnesium sulfate whisker, diameter 1.0 μm, L / D = 50, Kangru Technology Co., Ltd.

[0066] (6) GPM200A: maleic anhydride grafted polypropylene, melt flow rate: 144 g / 10 min (230°C, 2.16 kg), grafting rate: 0.8%, Ningbo Guangzhineng New Materials Technology Co., Ltd.;

[0067] (7) Polybond 7200: maleic anhydride grafted polypropylene, melt flow rate 250 g / 10 min (230 ° C, 2.16 kg), grafting rate 2.0%, Chemtura Corporation, USA;

[0068] (8) SEBS1657M: toughening agent, styrene-ethylene-butylene-styrene, melt flow rate 20 g / 10 min (230 °C, 2.16 kg), Kraton Polymers, USA;

[0069] (9) SEBS6014: toughening agent, styrene ethylene butylene styrene polymer, melt flow rate 5g / 10min (230℃, 2.16kg), Taiwan Rubber;

[0070] (10) SEBS7311F: toughening agent, styrene ethylene butylene styrene polymer, melt flow rate 1 g / 10 min (230 °C, 2.16 kg), Kuraray International Trading (Shanghai) Co., Ltd.;

[0071] (11) NX8000: transparent nucleating agent, Meiliken Chemical Co., Ltd.

[0072] (12) N04GT: transparent nucleating agent, Ningbo Hengze Chemical Co., Ltd.;

[0073] (13) SunShow1010: antioxidant, Lianlong New Materials Co., Ltd.

[0074] (14) SunShow168: Antioxidant, Lianlong New Materials Co., Ltd.

[0075] Other raw materials and reagents were purchased from commercial sources unless otherwise specified.

[0076] Preparation Example 1

[0077] The preparation method of modified magnesium sulfate whisker A is:

[0078] 1) Disperse 30 g of magnesium sulfate whisker WS-152 in 1500 g of deionized water, add 1.5 g of tetramethylammonium hydroxide (5%) of magnesium sulfate whisker, add dilute hydrochloric acid to adjust the pH to 5, react in a constant temperature water bath at 60° C. for 2 h, and obtain preliminary pre-dispersed magnesium sulfate whisker after suction filtration, washing and drying.

[0079] 2) 30 g of the pre-dispersed magnesium sulfate whiskers were dispersed in 1000 g of anhydrous ethanol solution, placed in an ultrasonic cleaning machine for ultrasonic treatment for 0.75 h, sodium dodecyl sulfate and γ-aminopropyltriethoxysilane were slowly added (wherein the mass ratio of pre-dispersed magnesium sulfate whiskers: sodium dodecyl sulfate: γ-aminopropyltriethoxysilane was 100:0.3:20), and placed in a constant temperature water bath at 70°C for reaction for 24 h. After filtration, washing and drying, modified magnesium sulfate whiskers A were obtained.

[0080] Preparation Example 2

[0081] The preparation method of modified magnesium sulfate whisker B is:

[0082] 1) Disperse 30 g of magnesium sulfate whisker WS-152 in 1500 g of deionized water, add 3 g of tetraethylammonium hydroxide (10% of the magnesium sulfate whisker), add dilute hydrochloric acid to adjust the pH to 6, react in a constant temperature water bath at 70° C. for 1 h, and obtain preliminary pre-dispersed magnesium sulfate whisker after suction filtration, washing and drying.

[0083] 2) 30 g of the preliminarily pre-dispersed magnesium sulfate whiskers were dispersed in 1000 g of anhydrous ethanol solution, placed in an ultrasonic cleaning machine for ultrasonic treatment for 0.45 h, sodium dodecyl sulfate and γ-aminopropyltriethoxysilane were slowly added (wherein the mass ratio of pre-dispersed magnesium sulfate whiskers: sodium dodecyl sulfate: γ-aminopropyltriethoxysilane was 200:0.2:15), and placed in a constant temperature water bath at 60°C for reaction for 12 h. After filtration, washing and drying, modified magnesium sulfate whiskers B were obtained.

[0084] Preparation Example 3

[0085] The preparation method of modified magnesium sulfate whisker C is:

[0086] 1) Disperse 30 g of magnesium sulfate whisker WS-152 in 1500 g of deionized water, add 2.4 g of tetrapropylammonium hydroxide (8%) of magnesium sulfate whisker, add dilute hydrochloric acid to adjust the pH to 4, react in a constant temperature water bath at 50° C. for 3 h, and obtain preliminary pre-dispersed magnesium sulfate whisker after filtration, washing and drying.

[0087] 2) 30 g of the preliminarily pre-dispersed magnesium sulfate whiskers were dispersed in 1000 g of anhydrous ethanol solution, placed in an ultrasonic cleaning machine for ultrasonic treatment for 0.25 h, sodium stearate and γ-aminopropyltriethoxysilane were slowly added (wherein the mass ratio of pre-dispersed magnesium sulfate whiskers: sodium stearate: γ-aminopropyltriethoxysilane was 150:0.1:25), and placed in a constant temperature water bath at 80°C for reaction for 18 h. After filtration, washing and drying, modified magnesium sulfate whiskers C were obtained.

[0088] Preparation Example 4

[0089] The preparation method of modified magnesium sulfate whisker D is basically the same as that of Example 1, except that the mass ratio of pre-dispersed magnesium sulfate whisker: sodium dodecyl sulfate: γ-aminopropyltriethoxysilane is 300:0.5:5.

[0090] Preparation Comparative Example 1

[0091] The preparation method of modified magnesium sulfate whisker E is:

[0092] 1) Disperse 30 g of magnesium sulfate whisker WS-152 in 1500 g of deionized water, add 1.5 g of tetramethylammonium hydroxide (5% of magnesium sulfate whisker), add dilute hydrochloric acid to adjust the pH to 5, react in a constant temperature water bath at 60° C. for 2 h, and obtain modified magnesium sulfate whisker E after suction filtration, washing and drying.

[0093] Preparation Comparative Example 2

[0094] The preparation method of modified magnesium sulfate whisker F is:

[0095] 1) 30 g of magnesium sulfate whisker WS-152 was dispersed in 1000 g of anhydrous ethanol solution, placed in an ultrasonic cleaning machine for ultrasonic treatment for 0.75 h, sodium dodecyl sulfate and γ-aminopropyltriethoxysilane were slowly added (wherein the mass ratio of magnesium sulfate whisker: sodium dodecyl sulfate: γ-aminopropyltriethoxysilane was 100:0.3:20), and placed in a constant temperature water bath at 70°C for reaction for 24 h, and the modified magnesium sulfate whisker F was obtained after filtration, washing and drying.

[0096] Example

[0097] The polypropylene material of the preparation example was prepared according to the ratio shown in Table 1 (the amount of each component in the table represents parts by weight), and the preparation process was as follows:

[0098] Weigh each raw material according to the weight portion described in the table below, and then put it into a high-speed mixer. After mixing the materials for a certain time and speed, put them into a twin-screw extruder, extrude and granulate them at the specified temperature and speed to obtain a polypropylene material.

[0099] Example 5 is basically the same as Example 1, except that the polypropylene used in Example 5 is all high-rigidity homopolymer polypropylene, and no random copolymer polypropylene is added.

[0100] Table 1 Raw material ratios and processing conditions of Examples 1 to 5

[0101]

[0102]

[0103] The polypropylene material of the comparative example was prepared according to the ratio shown in Table 2, and the preparation process was as follows: each raw material was weighed according to the weight portion as shown in Table 2, and then put into a high-speed mixer, after mixing the materials for a certain time and speed, put into a twin-screw extruder, and extruded and granulated at a specified temperature and speed to obtain a polypropylene material.

[0104] Comparative Example 1

[0105] This comparative example is substantially the same as Example 1, except that the modified magnesium sulfate whisker A is replaced by modified magnesium sulfate whisker E in this comparative example.

[0106] Comparative Example 2

[0107] This comparative example is substantially the same as Example 1, except that the modified magnesium sulfate whisker A is replaced by modified magnesium sulfate whisker F in this comparative example.

[0108] Comparative Example 3

[0109] This comparative example is substantially the same as Example 1, except that in this comparative example, the modified magnesium sulfate whisker A is replaced by unmodified magnesium sulfate whisker WS-152.

[0110] Comparative Example 4

[0111] This comparative example is substantially the same as Example 1, except that modified magnesium sulfate whisker A is not added in this comparative example, and is replaced by an equal amount of random copolymerized polypropylene 5012XT.

[0112] Comparative Example 5

[0113] This comparative example is substantially the same as Example 1, except that maleic anhydride grafted polypropylene is not added in this comparative example, and is replaced by an equal amount of random copolymerized polypropylene 5012XT.

[0114] Table 2 Raw material ratios and processing conditions of Comparative Examples 1-5

[0115]

[0116] The polypropylene materials obtained from Examples 1 to 5 and Comparative Examples 1 to 5 were subjected to performance tests, and the results are shown in Tables 3 and 4 below.

[0117] Table 3 Performance test results of various embodiments

[0118]

[0119] HDT stands for heat deformation temperature.

[0120] Table 4 Performance test results of each comparative example

[0121]

[0122] It can be seen from Comparative Example 4 that the mechanical properties of the polypropylene material without magnesium sulfate whiskers are very poor, and it can be seen from Comparative Example 3 that the mechanical properties of the polypropylene material with unmodified magnesium sulfate whiskers are improved, but its light transmittance is significantly reduced. Although the magnesium sulfate whiskers are modified to a certain extent in Comparative Examples 1 and 2, the improvement of light transmittance is limited.

[0123] From the data comparison of the embodiment and the comparative example, it can be seen that the optical performance of the present application is significantly improved compared with the comparative example, and its mechanical properties are also improved to a certain extent, while taking into account both mechanical properties and light transmittance.

[0124] By comparing Example 1 with Comparative Example 3 and Comparative Example 5, it can be seen that the rigidity, toughness, light transmittance, heat resistance and dimensional stability of the material in Example 1 are greatly improved, indicating that after the two-step modification, the -NH2 on the whiskers and the anhydride groups on the maleic anhydride grafted polypropylene undergo an interfacial compatibilization reaction, which greatly improves the dispersibility of the magnesium sulfate material in the material and the compatibility with the matrix.

[0125] By comparing Examples 1 to 3 with Example 4, it can be seen that when the mass ratio of the pre-dispersed magnesium sulfate whiskers, surfactant and γ-aminopropyltriethoxysilane is in the range of (100-200): (0.1-0.3): (15-25), the toughness and transmittance of the polypropylene material are higher.

[0126] By comparing Example 1 with Example 5, it can be seen that the toughness and light transmittance of the material can be further improved by compounding high-rigidity polypropylene with random copolymer polypropylene.

[0127] It can be seen from Table 3 that the polypropylene material prepared in the present invention has high light transmittance and high mechanical properties as well as high heat resistance.

[0128] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A polypropylene material, characterized in that: The raw materials include by weight: 40-90 parts of polypropylene, 0.5-5 parts of maleic anhydride grafted polypropylene, 5-15 parts of modified magnesium sulfate whiskers, 0.2-1.0 parts of transparent nucleating agent, 5-15 parts of toughening agent, 0.2-0.8 parts of antioxidant; The modified magnesium sulfate whisker is magnesium sulfate whisker modified by a dispersant, a surfactant and gamma-aminopropyltriethoxysilane.

2. The polypropylene material according to claim 1, characterized in that: The preparation method of the modified magnesium sulfate whisker comprises: S1: Mixing magnesium sulfate whiskers, water and a dispersant, adjusting the pH to 4-6, reacting, and then separating the solid from the liquid, washing and drying the solid to obtain pre-dispersed magnesium sulfate whiskers; S2: pre-dispersed magnesium sulfate whiskers, surfactants, γ-aminopropyltriethoxysilane and solvents are mixed, reacted, and then solid-liquid separation is performed, and the solid is washed and dried to obtain modified magnesium sulfate whiskers.

3. The polypropylene material according to claim 2, characterized in that: The preparation method of the modified magnesium sulfate whisker satisfies at least one of the following conditions: (1) In S2, the mass ratio of the pre-dispersed magnesium sulfate whiskers, the surfactant and γ-aminopropyltriethoxysilane is (100-300): (0.1-0.5): (5-25), preferably (100-200): (0.1-0.3): (15-25); (2) The reaction conditions of S2 are: reaction at a temperature of 60 to 80°C for 12 to 24 hours; (3) The reaction atmosphere of S2 is nitrogen; (4) the step of mixing the pre-dispersed magnesium sulfate whiskers, surfactant, γ-aminopropyltriethoxysilane and solvent in S2 comprises: firstly adding the pre-dispersed magnesium sulfate whiskers into the solvent for ultrasonic dispersion, and then adding the surfactant and γ-aminopropyltriethoxysilane; Optionally, the ultrasonic dispersion time is 0.25 to 0.75 h; Optionally, the solvent is anhydrous ethanol.

4. The polypropylene material according to claim 2, characterized in that: The preparation method of the modified magnesium sulfate whisker satisfies at least one of the following conditions: (1) In S1, the step of mixing magnesium sulfate whiskers, water and a dispersant comprises: adding magnesium sulfate whiskers to water for ultrasonic dispersion, and then adding a dispersant; Optionally, the ultrasonic dispersion time is 0.5 to 1.0 h; (2) The reaction conditions in S1 are 50-70°C for 1-3h; (3) In S1, the mass of the dispersant is 5.0-10.0% of the mass of the magnesium sulfate whiskers; (4) In S1, the aspect ratio of the magnesium sulfate whisker is greater than 30, and preferably the aspect ratio is 35-100.

5. The polypropylene material according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: (1) The dispersant is at least one selected from tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide; (2) The surfactant is at least one selected from sodium dodecyl sulfonate, sodium dodecyl sulfate and sodium stearate.

6. The polypropylene material according to any one of claims 1 to 4, characterized in that: The melt flow rate of the maleic anhydride grafted polypropylene is greater than 15 g / 10 min, and the maleic anhydride grafting rate is 0.5% to 2.0%.

7. The polypropylene material according to any one of claims 1 to 4, characterized in that: The polypropylene is selected from one or more of homopolypropylene and copolymer polypropylene; Optionally, the polypropylene is compounded by high rigidity homopolymer polypropylene and random copolymer polypropylene in a mass ratio of (30-50):(20-40); The high rigidity homopolymer polypropylene resin has a melt flow rate of 5 to 100 g / 10 min and a bending modulus of >1800 MPa; The random copolymer polypropylene is a polymer obtained by random copolymerization of propylene and ethylene, and has a melt flow rate of 1 to 10 g / 10 min.

8. The polypropylene material according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: (1) The transparent nucleating agent is selected from one or more of carboxylic acid metal salt nucleating agents, sorbitol nucleating agents, and aromatic phosphate nucleating agents; (2) The toughening agent is selected from one or more of vinyl-polydiene-styrene block copolymer, styrene-ethylene-butadiene-styrene copolymer, ethylene-octene copolymer, and ethylene-butene copolymer; (3) The antioxidant is selected from one or more of hindered phenol antioxidants, hindered amine antioxidants, phosphite antioxidants, thiodipropionate antioxidants, and thiol antioxidants, preferably hindered phenol antioxidants and phosphite antioxidants; Preferably, the mass ratio of hindered phenol antioxidant to phosphite antioxidant is (0.1-0.3):(0.1-0.3).

9. A method for preparing the polypropylene material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: Add various raw material components into a high-speed mixer according to the formula; S2: adding the premixed materials in step S1 into a twin-screw extruder, melt blending, extruding and granulating to obtain the polypropylene material; Optionally, the mixing condition of the high-speed mixer is 600 to 1000 r / min for 2 to 5 min; Optionally, the temperature of the twin-screw extruder is between 180° C. and 220° C., and the screw speed is between 500 and 900 r / min.

10. A bumper, characterized in that: The invention comprises the polypropylene material according to any one of claims 1 to 8 or the polypropylene material prepared by the method according to claim 9.

Citation Information

Patent Citations

  • Mineral / whisker reinforced polypropylene composite material having good spraying property

    CN101250303A

  • Polypropylene / inorganic whisker composite with enhanced flame resistance and preparation method thereof

    CN103509242A

  • Method for preparing polypropylene composite

    CN106854310A

  • High-surface-tension and low-density polypropylene composite material and preparation method thereof

    CN110951163A

  • High-strength plastic and processing technology thereof

    CN111849116A

Cited By

  • Polypropylene composite material as well as preparation method and application thereof

    CN119775660A