Low-hardness high-adsorption BIIR material, production process thereof and damping sucker

By using low hardness and high adsorption BIIR materials, the problem of thermoplastic elastomers becoming softened at high temperatures is solved. The material is made through a specific process, which increases adhesion and friction, and solves the stability and adsorption of suction cups at high temperatures. The effect extends the product life and improves the user experience.

CN119081302APending Publication Date: 2024-12-06ZHONGSHAN XIONGBING RUBBER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411328834.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-06

Smart Images

  • Figure BDA0005056212760000011
    Figure BDA0005056212760000011
  • Figure BDA0005056212760000021
    Figure BDA0005056212760000021
  • Figure BDA0005056212760000041
    Figure BDA0005056212760000041
Patent Text Reader

Abstract

The low-hardness high-adsorption BIIR material is prepared from the following components in parts by mass: 100 parts of butyl rubber, 5 to 30 parts of white carbon black, 20 to 80 parts of inorganic filler, 10 to 40 parts of softening agent, 3 to 5 parts of zinc oxide, 0.5 to 2 parts of magnesium oxide, 0.5 to 2 parts of stearic acid, 0.3 to 2 parts of wax, 2 to 15 parts of tackifying resin and 2 to 5 parts of accelerant. According to the low-hardness high-adsorption BIIR material, the high-airtight thermosetting characteristic of butyl rubber is utilized, deformation is not prone to occurring, the defects that a damping suction cup is prone to softening, poor in physical property and prone to falling off at the high temperature are overcome, high negative pressure of the suction cup is kept, the service life of a product is prolonged, stable performance of the suction cup is guaranteed, and the use experience of a user is improved; the tackifying resin is added into the BIIR material, so that the adhesive force of the sucker is increased, the sucker is easier to adhere to various interfaces, the friction force is improved, and the sucker is not easy to slide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer compound compositions, and in particular to a low-hardness, high-adsorption BIIR material and its production process, and a shock-absorbing suction cup. Background Art

[0002] Thermoplastic elastomer TPE / TPR, also known as artificial rubber or synthetic rubber, has the excellent properties of high elasticity, aging resistance and oil resistance of traditional cross-linked vulcanized rubber, while also having the characteristics of easy processing and wide processing methods of ordinary plastics.

[0003] Shock-absorbing suction cups utilize the high elasticity of thermoplastic elastomers and are usually used in the automotive and electrical appliance fields. However, in a high temperature environment, thermoplastic elastomers will become soft and their physical properties will deteriorate, resulting in a worse shock-absorbing effect of the shock-absorbing suction cup. The adsorption effect of the shock-absorbing suction cup may even deteriorate, causing the shock-absorbing suction cup to fall off the product, affecting the user experience of the shock-absorbing suction cup. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention proposes a low-hardness and high-absorption BIIR material, and the technical solution adopted includes:

[0005] A low hardness and high adsorption BIIR material, comprising, by weight:

[0006]

[0007]

[0008] A technical solution adopted by an embodiment of the present invention to solve the technical problem is: the tackifying resin is: phenolic resin.

[0009] The technical solution adopted by an embodiment of the present invention to solve the technical problem is: the accelerator is one or more of CBS, DM, TMTD and S.

[0010] A technical solution adopted by an embodiment of the present invention to solve the technical problem is: the softener is: polyisobutylene.

[0011] The present application also proposes a production process for the above-mentioned low hardness and high adsorption BIIR material, including:

[0012] Step 1, first put butyl rubber, white carbon black, inorganic filler, softener, magnesium oxide, stearic acid, wax, and tackifying resin into an internal mixer, mix and knead for 60-150 seconds, and the mixing temperature is 85°C; continue to mix and knead for 30-60 seconds after cleaning; then turn over and continue to mix and knead for 30-60 seconds;

[0013] Step 2, after completing step 1, continue to mix and heat to the mixing temperature of 115-150 ° C, unload and send to the open mixer, mix 3-4 times, and then cool to room temperature to obtain rubber A;

[0014] Step 3, add rubber compound A, accelerator and zinc oxide into the internal mixer, mix and knead for 60 seconds, turn over and clean the materials, and continue mixing and kneading for 60 seconds. After completion, continue to knead and heat to the internal mixing temperature of 90°C, pour out the rubber material and send it to the open mixer, adjust the roller distance of the open mixer to 1.5-3mm, turn over and discharge the sheet to obtain the finished product.

[0015] The technical solution adopted by an embodiment of the present invention to solve the technical problem is: in step 1, the step of turning over the sheets and continuing mixing and kneading for 30-60 seconds is repeated 1-2 times, and then step 2 is performed.

[0016] The present application also proposes a shock-absorbing suction cup, which is made of the low-hardness and high-absorption BIIR material as claimed in claim 1.

[0017] Beneficial effects of the present invention:

[0018] The high airtightness and thermosetting properties of butyl rubber make it difficult to deform, which solves the problem of the shock-absorbing suction cup becoming soft, deteriorating in physical properties and easily falling off under high temperatures. The suction cup maintains a high negative pressure, prolongs the product life, ensures stable suction cup performance and improves user experience.

[0019] Adding tackifying resin to BIIR material increases the adhesion of the suction cup, making it easier to adhere to various interfaces, and increases friction to prevent sliding. DETAILED DESCRIPTION

[0020] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art.

[0021] The present invention is further described in detail below in conjunction with specific examples and with reference to data. It should be understood that this embodiment is only for illustrating the present invention and is not intended to limit the scope of the present invention in any way.

[0022] In the following examples, various processes and methods not described in detail are conventional methods known in the art. The materials, reagents, devices, instruments, equipment, etc. used in the following examples, unless otherwise specified, can be obtained from commercial sources.

[0023] Comparative Example 1

[0024] In Comparative Example 1 of the present application, a shock-absorbing suction cup made of TPE material is used.

[0025] Example 1

[0026] Example 1 proposes a low-hardness and high-absorption BIIR material, which includes, by weight:

[0027]

[0028] Example 2

[0029] Example 2 proposes a low-hardness and high-absorption BIIR material, which includes, by weight:

[0030]

[0031]

[0032] Example 3

[0033] Example 3 proposes a low-hardness and high-absorption BIIR material, which includes, by weight:

[0034]

[0035] In this embodiment:

[0036] The production process of the low hardness and high adsorption BIIR material in Examples 1-3 includes:

[0037] Step 1, first put butyl rubber, white carbon black, inorganic filler, softener, magnesium oxide, stearic acid, wax, and tackifying resin into an internal mixer, mix and knead for 60-150 seconds, and the mixing temperature is 85°C; after cleaning, continue mixing and kneading for 30-60 seconds; then turn over the sheet and continue mixing and kneading for 30-60 seconds, and repeat turning over the sheet again and continue mixing and kneading for 30-60 seconds;

[0038] Step 2, after completing step 1, continue to mix and heat to the mixing temperature of 115-150 ° C, unload and send to the open mixer, mix 3-4 times, and then cool to room temperature to obtain rubber A;

[0039] Step 3, add rubber compound A, accelerator and zinc oxide into the internal mixer, mix and knead for 60 seconds, turn over and clean the materials, and continue mixing and kneading for 60 seconds. After completion, continue to knead and heat to 90°C, pour out the rubber material and send it to the open mixer, adjust the roller distance of the open mixer to 1.5-3mm, turn over the triangle bag 6 times and then take out the sheet to obtain the finished product.

[0040] In the embodiment, the tackifying resin is WSR2000 purchased from Jiangsu Ruiba New Material Technology Co., Ltd.; the accelerator is CBS; the softener is HRD-24 purchased from Shandong Hongrui New Material Technology Co., Ltd., with a molecular weight of 1000-5000.

[0041] The inorganic filler is talcum powder.

[0042] The finished products obtained in Examples 1-3 and the comparative example were compression molded to obtain shock-absorbing suction cups. The shock-absorbing suction cups obtained in Examples 1-3 and the comparative example were tested for physical properties. The test methods are shown in Table 1, and the test results are shown in Table 2.

[0043] Table 1

[0044]

[0045]

[0046]

[0047] Table 2

[0048]

[0049]

[0050] Of course, the present invention is not limited to the above-mentioned embodiments, and those skilled in the art may make equivalent modifications or substitutions without violating the spirit of the present invention. These equivalent modifications and substitutions are all included in the scope defined by the claims of this application.

Claims

1. A low hardness and high adsorption BIIR material, characterized in that: In terms of mass fractions, it includes:

2. The low hardness and high adsorption BIIR material according to claim 1, characterized in that: The tackifying resin is: phenolic resin.

3. The low hardness and high adsorption BIIR material according to claim 1, characterized in that: The accelerator is one or more of CBS, DM, TMTD and S.

4. The low hardness and high adsorption BIIR material according to claim 1, characterized in that: The softener is: polyisobutylene.

5. A production process of the low hardness and high adsorption BIIR material as claimed in claim 1, characterized in that: include: Step 1, first put butyl rubber, white carbon black, inorganic filler, softener, magnesium oxide, stearic acid, wax, and tackifying resin into an internal mixer, mix and knead for 60-150 seconds, and the mixing temperature is 85°C; continue to mix and knead for 30-60 seconds after cleaning; then turn over and continue to mix and knead for 30-60 seconds; Step 2, after completing step 1, continue to mix and heat to the mixing temperature of 115-150 ° C, unload and send to the open mixer, mix 3-4 times, and then cool to room temperature to obtain rubber A; Step 3, add rubber compound A, accelerator and zinc oxide into the internal mixer, mix and knead for 60 to 90 seconds, turn over and clean the materials, and continue mixing and kneading for 60 to 90 seconds. After completion, continue to knead and heat to the internal mixing temperature of 90 to 100°C, pour out the rubber material and send it to the open mixer, adjust the roller distance of the open mixer to 1.5-3mm, turn over and discharge the sheet to obtain the finished product.

6. The production process of low hardness and high adsorption BIIR material according to claim 5, characterized in that: In step 1, the process of turning over the sheets and mixing and kneading for 30-60 seconds is repeated 1-2 times, and then step 2 is performed.

7. A shock-absorbing suction cup, characterized in that: It is made of the low-hardness and high-absorption BIIR material as described in any one of claims 1 to 4.