Grain fiber / PVC (polyvinyl chloride) composite profile with high weather resistance

By adding specific ratios of PVC resin and nanocalcium powder to the rice husk powder imitation wood material, and performing surface activation treatment, combined with color coating technology, the problem of insufficient performance of rice husk powder imitation wood material in building doors and windows profiles is solved. , improves impact resistance and weather resistance, and realizes waste recycling and efficient production.

CN119081312APending Publication Date: 2024-12-06SHANGHAI QINGYING IND SHARES CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411406658.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When used in building doors and windows, the existing rice husk powder imitation wood materials have insufficient performance indicators, especially in terms of temperature changes and physical strength, they fail to meet the actual use requirements of building doors and windows. At the same time, a large amount of waste is generated during the production process. Lack of effective recycling programs.

Method used

A kind of ethylene method PVC resin containing 64-69%, 1-4% acrylate impact modifier, 0.5-2% HL processing aid, 0.1-0.5% oxidized polyethylene wax, 1- 5% compound calcium-zinc thermal stabilizer, 7-10% activated rice husk powder, 10-15% nano calcium powder, 2-6% modified toughener, 0.2-0.6% antioxidant, 0.3 -0.8% light stabilizer and 0.1-0.5% ultraviolet absorber, and improve the weather resistance of the profile by surface activation by rice husk powder and nanocalcium powder, combined with color coating technology, the weather resistance of the profile is improved by surface activation. and appearance quality.

Benefits of technology

It significantly improves impact resistance, welding and weather resistance, reduces profile costs, realizes effective recycling of waste, meets the high weather resistance requirements of building doors and windows profiles, and meets the needs of different users through color coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005076804300000091
    Figure BDA0005076804300000091
  • Figure BDA0005076804300000101
    Figure BDA0005076804300000101
Patent Text Reader

Abstract

The invention discloses a composition for manufacturing a grain fiber wood-like composite material used as a door and window profile. The composition comprises 64-69 wt% of ethylene-process PVC (polyvinyl chloride) resin; 1 to 4 wt% of an acrylate impact modifier; 0.5 to 2 wt% of an HL-based processing aid; 0.1 to 0.5 wt% of an external lubricant; 1-5 wt% of a composite calcium-zinc heat stabilizer; 7-10 wt% of activated rice hull powder; 10 to 15 weight percent of nano calcium powder; 2-6 wt% of a modified toughening agent; 0.2 to 0.6 wt% of an antioxidant; 0.3 to 0.8 wt% of a light stabilizer; 0.1 to 0.5 wt% of an ultraviolet absorber; and 7-10% by weight of recycled powder. The floor door and window profile prepared from the composition has high weather resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a grain fiber / PVC composite profile, and in particular to a grain fiber / PVC composite profile with high weather resistance. The profile can be used for building components, and in particular can be used as a profile for building doors and windows. The present invention also relates to a method for manufacturing the grain fiber / PVC composite profile. Background Art

[0002] In the context of the whole society emphasizing building energy conservation and green buildings, how to innovate and upgrade the technology on the basis of the original three basic materials of door and window materials: wood, plastic, and aluminum alloy, and launch a new type of building doors and windows that is resource-efficient, environmentally friendly, energy-saving, and green is a new attempt. The following is a specific description in sections.

[0003] Since 2012, the patented rice husk powder imitation wood material introduced from abroad has been made of environmentally friendly raw materials such as PVC resin and rice husks / peanut shells. Through a simple extrusion molding process, a high-grade imitation wood material with a very similar feel and processability to wood is prepared. At the same time, the color fastness and weather resistance of this imitation wood product are greatly enhanced compared to traditional wood-plastic composite materials. The imitation wood material "originates" from wood but is different from wood. It is free from the constraints of traditional wood and plastic, and has its own characteristics and excellent performance. It is "indistinguishable" from real wood in appearance, feel and use functions, and its service life is far longer than that of real wood. As a substitute for solid wood profiles, it is not only inexpensive but also can protect the ecological environment.

[0004] In response to the existing problems of WPC (wood plastic material), the applicant has improved the imitation wood material, using PVC resin to replace PE and PP resins, and using rice husk powder to replace sawdust as raw materials: the use of these raw materials is not subject to special restrictions, and even recycled PVC materials can be reused in the production and preparation of high-end imitation wood. In addition, the production and preparation of this imitation wood has no special restrictions on extrusion equipment, extrusion methods, and the order of adding raw materials. This is ahead of conventional wood-plastic composite materials in terms of production flexibility and product diversity, and the shape of the profile is extremely convenient to adjust. At present, after years of product research and development and market practice in the Chinese market from Germany, the processed products are still in the application of indoor and outdoor building decoration materials and outdoor furniture materials.

[0005] From the above analysis, rice husk powder imitation wood material is indeed a good product in the architectural decoration and furniture industries. It can be widely used in indoor and outdoor floors, waterside pedals, garden decoration, outdoor furniture and other products.

[0006] However, from the perspective of the entire domestic market and even the global market, there is no precedent for applying this material to building components, especially building door and window profiles with high weather resistance requirements. To this end, we should make full use of the various properties and characteristics of this material, and overcome some technical deficiencies in the physical index testing of door and window profiles. In the application field of building door and window profiles, we should retain some advantages of the original rice husk powder imitation wood material, and re-develop a new set of application technologies to meet the needs of the corresponding market and industry, and make a rational comparison with traditional door and window profiles on the market in terms of performance, texture, benefits, etc., and find that it has greater technical advantages and is closer to the actual needs of direct users and the market.

[0007] From the analysis of current market applications, this type of imitation wood material has some deficiencies in profile product performance indicators, which have been explained before. In particular, in terms of deformation caused by temperature changes and physical strength indicators, there is a certain gap between them and the actual use requirements of building doors and windows.

[0008] In addition, under the condition that the profile body is in reasonable weather resistance index, it is also necessary to colorize the two visible surfaces inside and outside the profile.

[0009] Furthermore, a large amount of waste is generated during the production process of existing imitation wood materials. Recycling and reusing these wastes is also in line with the concept of green environmental protection. Summary of the invention

[0010] The technical problem to be solved by the present invention is to provide an improved corn fiber imitation wood composite material composition for door and window profiles, which has high weather resistance.

[0011] In order to solve the above technical problems, the present invention provides a composition for manufacturing a corn fiber imitation wood composite material used as a door and window profile, the composition comprising: 64-69 weight % of ethylene-based PVC resin; 1-4 weight % of acrylate impact modifier; 0.5-2 weight % of HL processing aid; 0.1-0.5 weight % of external lubricant oxidized polyethylene wax; 1-5 weight % of composite calcium zinc heat stabilizer; 7-10 weight % of activated rice husk powder; 10-15 weight % of nano calcium powder; 2-6 weight % of modified toughening agent; 0.2-0.6 weight % of antioxidant; 0.3-0.8 weight % of light stabilizer; 0.1-0.5 weight % of ultraviolet absorber; and 7-10 weight % of recycled powder, wherein the combined light stabilizer includes light stabilizer 770 and ultraviolet absorber UVP327; the rice husk powder is 60 The invention discloses a method for preparing a rice husk powder comprising the steps of: a1) screening, washing, drying and crushing the rice husk; a2) screening the rice husk powder crushed in step a1) for the second time and sieving to obtain two finished powders with fineness of 80-100 mesh and 60 mesh; a3) adding the two rice powders with different meshes into a high-speed mixer according to the above proportion, stirring at a high speed of 950-1000 rpm to 80-100° C., adding a coupling agent, continuing to stir to 120° C., and discharging the mixture out of the pot and entering a cold mixing device to reduce the temperature to less than 50° C.; in the above surface activation treatment, the coupling agent is powdery and is selected from at least one of aluminates, silanes and titanates; and the nano calcium powder is a nano light calcium carbonate with a mesh of 3000-4500 mesh.

[0012] Preferably, the composition comprises: 65-67 wt % of ethylene-based PVC resin; 2-3 wt % of acrylate impact modifier; 0.8-1.5 wt % of HL processing aid; 0.2-0.4 wt % of oxidized polyethylene wax; 2-4 wt % of composite calcium zinc heat stabilizer; 7-9 wt % of activated rice husk powder; 11-13 wt % of nano calcium powder; 3-5 wt % of modified toughening agent; 0.3-0.5 wt % of antioxidant; 0.4-0.6 wt % of light stabilizer; 0.2-0.4 wt % of ultraviolet absorber; 0.1-0.5 wt % of external lubricant; and 8-9 wt % of recycled powder.

[0013] Preferably, the preparation method of the composition comprises the following steps: a) pouring PVC resin, rice husk powder and nano calcium powder into a mixer and mixing at a low speed of 400-450 rpm for 3-5 minutes; b) pouring acrylate impact modifier, HL processing aid, external lubricant, composite calcium zinc heat stabilizer, modified toughening agent, antioxidant, light stabilizer, ultraviolet absorber, and recycled powder into the mixer and mixing at a high speed of 950-1000 rpm so that the material reaches 125°C; c) continuing to stir at a low speed for 6-8 minutes under the condition of 125°C, and then discharging the material into a cooling mixer; d) when the material is stirred and cooled to 45-50 degrees in the cooling mixer, all of it is discharged and packed into a moisture-proof bag for standby use, and the water content of the material is kept below 1%.

[0014] Preferably, the acrylic ester impact modifier is P335.

[0015] Preferably, the modified toughening agent is an ACM (Acrylate Copolymer Modified) impact toughening agent.

[0016] Preferably, the external lubricant is oxidized polyethylene wax.

[0017] According to another aspect of the present invention, a coating process for door and window profiles made of the above-mentioned composition is also proposed, which includes the following steps: grinding the profile surface with an abrasive belt with a mesh size of 60 and / or 120, and polishing after grinding; coating the treated profile surface with UV paint, wherein the UV paint includes: UV adhesion primer; UV color paint; a first UV aging-resistant topcoat; and a second UV aging-resistant topcoat.

[0018] Preferably, the above-mentioned coating process, wherein: the above-mentioned coating is divided into six layers or more for coating and drying, the surface of the profile is polished again before painting, and the amount of paint per layer is 10-22 g / m2; the 1st-2nd layers of paint should be applied to the surface with a brush to ensure uniform coating of the paint, and the dryness is controlled at 50%-75%; the 3rd-4th layers of UV color paint, if it is a wood grain surface, only the 3rd layer is coated with a brush; if it is a full glossy surface, the 3rd and 4th layers are coated without a brush, and the dryness is controlled at 75%; the 5th layer of UV topcoat does not use a brush, the paint brightness is 30%±3, and the dryness is 75%; the 6th layer of UV topcoat does not use a brush, the paint brightness is 15%±3, and the dryness is 100%.

[0019] The present invention has the following advantages.

[0020] 1. The grain fiber imitation wood products made of the composition of the present invention have better performance than existing products in terms of impact resistance, weldability and other aspects.

[0021] 2. The present invention adopts a reasonable addition ratio of calcium carbonate and rice husk powder, and adds them into the formula for application, which achieves an excellent process adaptation effect, and also increases the hardness and rigidity of the profile product. And the cost of the rice husk powder filled profile is controlled within a certain reasonable range, creating a stable and good economic benefit.

[0022] 3. Adding heat stabilizer and combined light stabilizer to the formula makes the product resistant to light and heat erosion and has excellent weather resistance.

[0023] 4. The present invention also includes a color coating process, in which the profiles made of the above composition are processed through the color coating process to produce various colored profiles. DETAILED DESCRIPTION

[0024] The present invention is a composition for manufacturing a grain fiber imitation wood composite material. In one embodiment, the composition of the present invention comprises: 64-69 weight percent of ethylene-based PVC resin; 1-4 weight percent of acrylate impact modifier; 0.5-2 weight percent of HL processing aid; 0.1-0.5 weight percent of 316A external lubricant, preferably oxidized polyethylene wax; 1-5 weight percent of composite calcium zinc heat stabilizer; 7-10 weight percent of activated rice husk powder; 10-15 weight percent of nano calcium powder; 2-6 weight percent of modified toughening agent; 0.2-0.6 weight percent of antioxidant; 0.3-0.8 weight percent of light stabilizer; 0.1-0.5 weight percent of ultraviolet absorber, and 7-10 weight percent of recycled powder.

[0025] In a preferred embodiment, the above composition comprises: 65-67 weight % of PVC resin; 2-3 weight % of acrylate impact modifier; 0.8-1.5 weight % of HL processing aid; 0.2-0.4 weight % of 316A lubricant; 2-4 weight % of composite calcium zinc heat stabilizer; 7-9 weight % of activated rice husk powder; 11-13 weight % of nano calcium powder; 3-5 weight % of modified toughening agent; 0.3-0.5 weight % of antioxidant; 0.4-0.6 weight % of light stabilizer; 0.2-0.4 weight % of ultraviolet absorber, and 8-9 weight % of recycled powder.

[0026] The light stabilizer is Light Stabilizer 770, and the ultraviolet absorber is UVP327. The nano calcium powder is a nano light calcium carbonate with a mesh number of 3000-4500 meshes.

[0027] In the above formula, rice husk powder is used as the first filler and calcium carbonate is used as the second filler, and surface treatment is required. Since the filling amount of these two substances is relatively large, they will have a great impact on the plasticization and processing properties of the raw materials. The surface polarity of untreated rice husk powder and calcium carbonate is very strong, and the oil absorption is very poor, so the compatibility with PVC resin is very poor. At the same time, there is no affinity for various stabilizers, internal and external lubricants and other processing aids in the formula, which makes extrusion molding difficult. Therefore, the active modification process of its surface is very necessary.

[0028] Rice husk powder is the main byproduct of rice processing. In addition to lignin and wood fiber, it also contains 15-20% amorphous silica. However, rice husk powder has a big weakness, which is strong hydrophilicity, that is, the raw material is more susceptible to moisture, which causes certain difficulties in extrusion processing and raw material storage. The surface lipophilicity of the filler is relatively weak, so it has a negative effect on the compatibility of the polymer material of the main carrier of the raw material.

[0029] The surface activation treatment of rice husk powder is described as follows. Since some coupling agents are in liquid state, it is difficult to spray them evenly on the surface of the raw material during high-speed stirring. Therefore, the present invention uses a powdered coupling agent. Specifically, a powdered coupling agent, such as aluminates, silanes, and titanates, is stirred at high speed with rice husk powder so as to be evenly sprayed on the surface of the raw material, and a set of feasible processing routes is determined to obtain an activated powder that meets the use requirements. The above-mentioned coupling agent preferably uses a powdered phthalate coupling agent.

[0030] First, the rice husks are screened to remove platycodon and impurities, then they are washed several times and dried by hot air. When the moisture is controlled within 2%, they are crushed and screened for the second time. The finished powder is sieved to separate the fineness into 80-100 mesh and 60 mesh, and then packaged and bagged for short-term storage.

[0031] The moisture content of the rice powder treated by the surfactant process should be controlled within 1.5%. If necessary, secondary drying treatment should be carried out. Two different mesh rice powders are added into a high-speed mixer (with a heating device) according to the specified proportion, such as 40% for 60 mesh and 60% for 80-100 mesh. When the high-speed stirring reaches 80-100 degrees, a coupling agent in an appropriate proportion is added, and stirring is continued until about 120 degrees. The material is discharged from the pot and put into the cold mixing equipment. When the temperature of the raw materials drops to less than 50 degrees, the material is discharged from the pot and bagged according to the specified weight for standby use. The packaging bag adopts waterproof packaging.

[0032] In addition, calcium carbonate uses nano-type active light calcium carbonate products with good dispersibility and mesh size of 3000-4500 as the second filler. It forms a reasonable addition ratio with rice husk powder and is added to the formula for application, which has achieved excellent process adaptation effect, and also increased the hardness and rigidity of the profile product. It also controls the cost of rice husk powder filled profiles within a certain reasonable range, creating stable and good economic benefits.

[0033] According to the determination of the connection process and strength of the profile corners, the welding quality of the door and window corners is a relatively critical issue. In addition to solving the problem of corner leakage, the strength of the weld corner itself should also be guaranteed to meet the current door and window standards and profile standards, including the requirements for weld corner strength that have been issued and implemented by the group standard T / CECS10175-2022 "Grain Fiber Composite Doors and Windows for Construction", the failure stress of the weld corner shall not be less than 30mpa / mm 2 . In the initial formulation test, due to the compatibility problem of the internal and external lubricant systems in the formulation, the lubricant had the phenomenon of surface precipitation. At the same time, the impact resistance system of the CPE originally used in the material also had some ratio combination problems, resulting in poor weld angle strength indicators, and the direction of weld cracking after the weld angle was damaged was also wrong. The formulation of the present invention uses 316a as a lubricant, and selects a reasonable combination of acrylate impact modifiers and toughening agents. Through multiple adjustments to the ratio of the impact resistance system and the internal and external lubrication system, the expected technical requirements are met. Through testing, a good weld angle destructive force effect is obtained. The newly determined standard value is: 30MPa, and the average value (5 test pieces) reaches 42MPa, and the minimum destructive force also obtains a result of 38MPa.

[0034] Since the door and window profile is a kind of building component used outdoors, it should have excellent weather resistance while having good physical indicators. The formation of this aging mechanism is caused by the erosion of light and heat. First of all, there are also requirements for aging and discoloration in existing imitation wood products, but those are technical data, testing standards and operating methods for building decoration materials, which are very different from the physical technical indicators of building exterior door and window profiles. The applicant refers to some technical requirements of the latest European U-PVC profile standard (EN12608-2016), and also strictly implements the product standard T / TECS10175-2022 of our company's doors and windows for artificial aging indicators and testing methods for outdoor door and window profiles to develop the special weather resistance formula of the door and window profile of the present invention.

[0035] First of all, in terms of thermal stability, in addition to resisting the problem of heat on the outer surface of the profile caused by natural sunlight, more importantly, the secondary high temperature generated during the extrusion production process and the door and window welding process causes overall or partial discoloration and decomposition of the material itself. Ensuring good thermal stability is an important link.

[0036] In the prior art, the heat stabilizer uses lead salt stabilizer (metal soap), which is a commonly used stabilizer with good thermal stability, wide processing range, excellent electrical properties, low price, etc. However, it contains a relatively high lead component and is a polluting stabilizer, which does not meet environmental protection requirements, especially the requirements of green building materials.

[0037] In the present invention, a composite calcium-zinc heat stabilizer is used, which is a non-toxic, environmentally friendly heat stabilizer, and has the advantages of excellent initial coloring, strong weather resistance, reasonable price, easy dispersion, good compatibility with PVC, good lubricity, etc. The internal structure of the profile for grain fiber / PVC doors and windows produced by using composite calcium-zinc is finer than that produced by using lead salt, and the calcium-zinc stabilizer also has the functions of coupling, strengthening and brightening in polyvinyl chloride (PVC) materials. In addition, the calcium-zinc composite stabilizer also has the functions of enhancing color, toughening, increasing volume and weather resistance, and its insulation is excellent. Therefore, the surface texture of the profile is better and the cross section is more uniform.

[0038] In order to make the profile body have perfect weather resistance, various additives that absorb and block ultraviolet rays must be added, and first of all, light-stabilizing additives must be selected. In the present invention, the light stabilizer is a combination of light stabilizer 770 and UVP-327.

[0039] Light stabilizer 770 (LS-770), also known as low molecular weight hindered amine light stabilizer 770, absorbs or reflects ultraviolet rays, reduces the speed of photothermal decomposition, and prolongs the service life of the product. In the present invention, light stabilizer 770 is added to the PVC / grain fiber composite material to improve the weather resistance and long-term service life of the material.

[0040] UV absorber UVP-327 is also a light stabilizer that can absorb the ultraviolet part of sunlight and fluorescent light sources without changing itself. Plastics and other polymer materials produce auto-oxidation reactions under sunlight and fluorescence due to the action of ultraviolet rays, which leads to the degradation and deterioration of polymers, and the deterioration of appearance and mechanical properties. After adding ultraviolet absorbers, this high-energy ultraviolet light can be selectively absorbed, turning it into harmless energy and releasing or consuming it. Ultraviolet absorbers should meet the following conditions:

[0041] ① It can strongly absorb ultraviolet rays (especially ultraviolet rays with a wavelength of 290-400nm); ② It has good thermal stability and will not change due to heat even during processing, and has low thermal volatility; ③ It has good chemical stability and will not react adversely with the material components in the product; ④ It has good miscibility and can be evenly dispersed in the material without frost or seepage; ⑤ The absorbent itself has good photochemical stability, does not decompose, and does not change color; ⑥ It is colorless, non-toxic, and odorless; ⑦ It is resistant to immersion and washing; ⑧ It is cheap and easy to obtain.

[0042] UVP-327 is suitable for various plastics such as polyvinyl chloride, polyvinylidene chloride, polymethyl methacrylate, unsaturated polyester, ABS resin and cellulose resin. It hardly absorbs visible light, so it is suitable for light-colored transparent products. UV absorber UVP-327 is an excellent and efficient UV absorber, mainly used to enhance the aging resistance of composite materials. Its main functions are reflected in the following aspects:

[0043] 1. Highly efficient absorption of ultraviolet rays: UVP-327 can strongly absorb ultraviolet rays with a wavelength of 240-340 nanometers, especially in the range of 270-330 nanometers. This feature enables it to effectively protect polymer materials such as PVC from ultraviolet damage.

[0044] 2. Reduce color changes: UVP-327 not only absorbs ultraviolet rays, but also helps reduce the color changes of polymers caused by ultraviolet rays and delays the yellowing of materials.

[0045] 3. Delaying the loss of physical properties: By absorbing ultraviolet rays, UVP-327 can delay the loss of physical properties of PVC materials, such as cracking and aging, thereby extending the service life of the material.

[0046] 4. Excellent compatibility and low volatility: UVP-327 has good compatibility with resin materials such as PVC and low volatility. The general dosage is between 0.1% and 1%, and it is easy to process and apply.

[0047] 5. Environmental protection and safety: UVP-327 is light in color and non-toxic. Many countries allow it to be used in plasticized products that come into contact with food, demonstrating its environmental protection and safety.

[0048] Ultraviolet absorber UVP-327 can significantly improve the aging resistance and service life of the material. In the test of the grain fiber / PVC composite material of this application, repeated comparisons were made. First, the effect performance is good, second, the cost is low, and third, the process adaptability is good. The combination of light stabilizer 770 and UVP-327 makes the existing production formula more reasonable and effective.

[0049] After many times of variety screening and adjustment of addition amount, and through the adaptability of batch tests and verification of testing, the quality standard of building exterior window profiles specified in the standard and artificial aging test ≥4000 hours have been achieved. The appearance and strength of the profiles after artificial aging meet the technical requirements. At the same time, they have passed the test of door and window processing and fully meet the welding process and mass production requirements of Valley Fiber door and window profiles.

[0050] Through physical testing of the original wood-like formula material, we found that it is hard, with good rigidity and bending resistance. The corresponding problem is that it is very brittle, especially with poor impact resistance under low temperature conditions. As building door and window profiles used outdoors, especially in northern China, the profile standards have very strict requirements on technical indicators in this regard, including low-temperature drop hammer impact test and welding strength test. Furthermore, if the impact resistance is not good, the profile will collapse and weld stress cracking will occur during the processing and production of doors and windows in winter. When installing doors and windows at low temperatures, the welds and windows will also be damaged due to external forces. After repeated tests of a variety of low-temperature resistant impact modifiers, including CPE system, acrylate system, and ABS impact system, the technology of blending acrylate impact modifiers with impact (toughening agent) was finally selected, which achieved good application results.

[0051] In the original profile formula, the traditional CPE+toughener blending technology in the industry was used in low-temperature impact resistance. The physical test indicators were very unstable and substandard phenomena occurred from time to time. In order to stabilize the process and improve the stability of quality, after repeated comparative tests, this patent used the latest impact resistance system, and the cost was reduced, with good results. The following analysis and introduction:

[0052] Acrylate impact modifiers (P355) are a class of chemicals used to improve the impact resistance of polymer materials. They mainly improve the toughness and impact strength of materials through specific chemical structures and formula designs. The following are some of the main types of acrylate impact modifiers and their functions:

[0053] 1. Improve impact resistance: Acrylic impact modifier can effectively absorb impact energy and prevent crack expansion when subjected to external impact through its specific core-shell structure, thereby significantly improving the impact resistance of the material.

[0054] 2. Improve processing performance: Some acrylic impact modifiers can also improve the processing performance of plastics, such as increasing fluidity, reducing processing temperature, etc., making the processing process smoother and more efficient.

[0055] 3. Enhanced weather resistance: Some acrylic impact modifiers have excellent weather resistance and can resist the erosion of environmental factors such as ultraviolet rays, high temperature, and humidity, thus extending the service life of the material.

[0056] 4. Improve toughness: By improving the toughness of the material, acrylic impact modifiers can make PVC profile products less likely to break or deform when subjected to external forces, thereby improving the overall quality and safety of the product.

[0057] In addition, the toughening system used in conjunction with it adopts ACM (Acrylate Copolymer Modified) impact toughening agent.

[0058] ACM impact toughener has excellent low-temperature toughness, which can significantly improve the performance of PVC profiles in low-temperature environments and prevent damage caused by brittle fracture. This feature is particularly important in cold regions or in applications that need to withstand low-temperature impact.

[0059] The CPE in ACM products works together with the acrylic polymer to make its elongation at break far exceed that of general materials, thereby effectively absorbing and dispersing impact energy and protecting the product from damage.

[0060] ACM impact toughener not only enhances the toughness of PVC profiles, but also gives them better processing performance. During the processing, ACM can reduce the amount of processing aids, reduce production costs and improve production efficiency.

[0061] ACM has good compatibility with PVC materials and can be evenly dispersed in the PVC matrix to form a stable toughening system, ensuring the uniformity and stability of product performance.

[0062] In this case, this patent uses acrylic anti-impact agent (P355) in combination with ACM toughening agent to obtain relatively stable physical test indicators.

[0063] The specific method for preparing the grain fiber imitation wood composite material composition is described below, and the method comprises the following steps:

[0064] a) Pour PVC resin, rice husk powder and nano calcium powder into a mixer and mix at a low speed of 400-450 rpm for 3-5 minutes;

[0065] b) pouring the acrylic impact modifier, HL processing aid, oxidized polyethylene wax, composite calcium zinc heat stabilizer, modified toughening agent, antioxidant, light stabilizer, ultraviolet absorber, and recycled powder into the mixer and mixing at a high speed of 950-1000 rpm until the material reaches 125° C.;

[0066] c) Continue stirring at low speed for 6 to 8 minutes at 125°C and then discharge the material into a cooling mixer;

[0067] d) When the materials are stirred and cooled to 45-50 degrees in the cooling mixer, they are all released and put into moisture-proof bags for standby use, and the moisture content of the materials is kept below 1%.

[0068] More specifically, the above step a) may also include:

[0069] In this embodiment, rice powder with a fineness of 100 mesh is used for surface activation treatment, which includes the following steps:

[0070] a1) screening, washing, drying and then crushing the rice husks;

[0071] a2) screening the rice husk powder after the crushing in step a1) for a second time, and sieving to obtain a finished powder with a fineness of 100 mesh;

[0072] a3) Add the finished powder into a high-speed mixer and stir at 950-1000 rpm until the temperature reaches 80-100°C. Then add the coupling agent and continue stirring until the temperature reaches 120°C. Remove the powder from the pot and discharge it into a cold mixing equipment to reduce the temperature to less than 50°C.

[0073] In the above surface activation treatment, the coupling agent is in powder form and is selected from at least one of aluminates, silanes and titanates; the nano calcium powder is nano light calcium carbonate with a mesh size of 3000-4500 meshes.

[0074] The finished powder can be dried a second time before adding the coupling agent.

[0075] The recycled powder in this embodiment is waste material recycled and reused in the previous material production process.

[0076] According to the above method, the composition of the present invention can be obtained as follows.

[0077] Example 1

[0078] The invention discloses a composition for manufacturing a rice fiber imitation wood composite material, comprising 64 weight percent of ethylene-based PVC resin, 1.5 weight percent of acrylate impact modifier, 0.9 weight percent of HL processing aid, 0.5 weight percent of oxidized polyethylene wax, 1 weight percent of composite calcium-zinc heat stabilizer, 8 weight percent of activated rice husk powder, 10 weight percent of nano-calcium powder, 4 weight percent of modified toughening agent, 0.2 weight percent of antioxidant, 0.8 weight percent of light stabilizer, 0.1 weight percent of ultraviolet absorber and 9 weight percent of recycled powder.

[0079] The average value of the weld corner destructive force test (5 specimens) was 37.5MPa, and the minimum destructive force was 34.5MPa.

[0080] Example 2

[0081] The invention discloses a composition for manufacturing a rice fiber imitation wood composite material, comprising 65 weight percent of ethylene-based PVC resin, 2 weight percent of acrylate impact modifier, 0.5 weight percent of HL processing aid, 0.2 weight percent of oxidized polyethylene wax, 1 weight percent of composite calcium-zinc heat stabilizer, 9 weight percent of activated rice husk powder, 11 weight percent of nano calcium powder, 3 weight percent of modified toughening agent, 0.2 weight percent of antioxidant, 0.5 weight percent of light stabilizer, 0.1 weight percent of ultraviolet absorber and 7.5 weight percent of recycled powder.

[0082] The average value of the weld corner destructive force test (5 specimens) was 39.6MPa and the minimum destructive force was 36.1MPa.

[0083] Example 3

[0084] The invention discloses a composition for manufacturing a rice fiber imitation wood composite material, comprising 66 weight percent of ethylene-based PVC resin, 2.5 weight percent of acrylate impact modifier, 0.2 weight percent of oxidized polyethylene wax, 1 weight percent of composite calcium-zinc heat stabilizer, 9 weight percent of activated rice husk powder, 11 weight percent of nano-calcium powder, 3 weight percent of modified toughening agent, 0.2 weight percent of antioxidant, 0.5 weight percent of light stabilizer, 0.1 weight percent of ultraviolet absorber, and 7.5 weight percent of recycled powder.

[0085] A low-temperature drop hammer impact test was conducted with an impact height of 1.2 meters. There were 10 specimens and two of them broke.

[0086] Example 4

[0087] The invention discloses a composition for manufacturing a grain fiber imitation wood composite material, comprising 67 weight percent of ethylene-based PVC resin, 2 weight percent of acrylate impact modifier, 0.5 weight percent of HL processing aid, 0.2 weight percent of oxidized polyethylene wax, 2 weight percent of composite calcium-zinc heat stabilizer, 6 weight percent of activated rice husk powder, 12 weight percent of nano calcium powder, 5 weight percent of modified toughening agent, 0.2 weight percent of antioxidant, 0.5 weight percent of light stabilizer, 0.1 weight percent of ultraviolet absorber and 7.5 weight percent of recycled powder.

[0088] A low-temperature drop hammer impact test was conducted with an impact height of 1.5 meters. Ten specimens were tested and one was broken.

[0089] In addition, according to the requirements of product appearance and texture, it is necessary to colorize the two visible surfaces of the profile under the condition that the profile body is in a reasonable weather resistance index. Therefore, the present invention also includes a color coating process, and the profile made of the above composition is made into various colored profiles through a color coating process.

[0090] The composition ratios of the color coating material of the present invention are shown in the following table, wherein the ratios are in weight %.

[0091]

[0092]

[0093] The specific coating processes and coating materials are listed as follows:

[0094] 1) Surface grinding process of profiles

[0095] Use special grinding equipment to grind the surface of profiles with different cross sections. Use abrasive belts with different surface coarseness and fineness according to company regulations or customer requirements. Commonly used abrasive belt mesh: 60# and / or 120#. After grinding, the surface needs to be polished and cleaned. This production process uses a scouring pad roller and a DuPont silk roller. The purpose of grinding is to form different coarse and fine wood textures to fully reflect the realistic effect of the product imitating wood, and to remove the original skin through process treatment to form a new grinding layer, thereby increasing the adhesion of paint on the surface of the profile and meeting the product quality requirements.

[0096] 2) Regulations on UV paint coating materials

[0097] First of all, UV adhesion primer is the key to ensure the bonding adhesion between the profile surface and the paint layer. UV transparent sanding primer (to ensure proper filling of the surface).

[0098] UV paint: Make the product have a variety of colors for different customers to choose from, preferably 8 different colors.

[0099] UV resistant topcoat (first layer of topcoat).

[0100] UV resistant topcoat (second layer of topcoat).

[0101] The second layer of topcoat ensures that the product's artificial aging test is ≥6000 hours, and the surface brightness is (20%-30%).

[0102] 3) UV paint coating process regulations

[0103] 3a) The product is painted and dried in six or more layers depending on the surface requirements of the product.

[0104] 3b) Polish the profile surface again before painting (Dupont roller plus sandpaper strip roller). Then paint five or six times, with each layer of paint using 10-22 g / m2.

[0105] 3c) The first and second coats of paint should be applied with a brush to ensure even coating of the paint and control the dryness at 50%-75%.

[0106] 3d) The 3rd-4th layers of UV paint are divided into wood grain surface and full gloss surface according to the product appearance texture requirements.

[0107] When it is a wood grain surface, the product is only applied in the third coat, using a brush;

[0108] When applying the 3rd and 4th layers of full-gloss products, do not use a brush and control the dryness at 75%.

[0109] 3e) The fifth layer of UV topcoat is applied without a brush, the paint gloss is 30% ± 3, and the dryness is 75%.

[0110] 3f) The 6th layer of UV paint is applied without a brush, the paint brightness is 15% ± 3, and the dryness is 100%.

[0111] After the two visible surfaces are polished and painted, they are tested for artificial aging and weather resistance. The aging time should be ≥ 6000 hours, and all technical indicators should meet the standard technical requirements.

[0112] Through this process, the needs of different users for coloring doors and windows can be met. In addition, the profile surface has a higher weather resistance (aging resistance) performance, which can ensure that the service life of doors and windows matches that of buildings.

[0113] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A composition for making a corn fiber imitation wood composite material used as a door and window profile, It is characterized in that The composition comprises: 64-69 wt% ethylene-based PVC resin; 1-4 wt % acrylate impact modifier; 0.5-2 wt% of HL processing aid; 0.1-0.5 wt% external lubricant; 1-5 wt% of a composite calcium zinc heat stabilizer; 7-10 wt% activated rice husk powder; 10-15% by weight of nano calcium powder; 2-6 wt% of a modifying toughening agent; 0.2-0.6 wt% antioxidant; 0.3-0.8 wt% of light stabilizer; 0.1-0.5 wt % of a UV absorber; and 7-10% by weight of recycled powder, in, The combined light stabilizer includes light stabilizer 770 and ultraviolet absorber UVP327; The rice husk powder is mixed at 40% of 60 mesh and 60% of 80-100 mesh; and the rice husk powder is subjected to surface activation treatment, and the surface activation treatment comprises the following steps: a1) screening, washing, drying and then crushing the rice husks; a2) screening the rice husk powder after the crushing in step a1) for a second time, and sieving to obtain two kinds of finished powders with fineness of 80-100 mesh and 60 mesh; a3) adding two kinds of rice flour with different mesh sizes into a high-speed mixer according to the above proportion, stirring at 950-1000 rpm to 80-100° C., adding a coupling agent, continuing to stir to 120° C., and discharging the mixture out of the pot into a cold mixing equipment to reduce the temperature to less than 50° C.; In the above surface activation treatment, the coupling agent is in powder form and is selected from at least one of aluminates, silanes, and titanates; The nano calcium powder is nano light calcium carbonate with a mesh size of 3000-4500 meshes.

2. The composition according to claim 1, It is characterized in that The composition comprises: 65-67% by weight of ethylene-based PVC resin; 2-3 wt% acrylate impact modifier; 0.8-1.5 wt% of HL processing aid; 0.2-0.4 wt% external lubricant; 2-4 wt% of a composite calcium zinc heat stabilizer; 7-9 wt% activated rice husk powder; 11-13% by weight of nano calcium powder; 3-5 wt% of a modifying toughening agent; 0.3-0.5 wt% antioxidant; 0.4-0.6 wt% of light stabilizer; 0.2-0.4 wt % of a UV absorber; and 8-9 wt% recycled powder.

3. The composition according to claim 1, It is characterized in that The preparation method of the composition comprises the following steps: a) Pour PVC resin, rice husk powder and nano calcium powder into a mixer and mix at a low speed of 400-450 rpm for 3-5 minutes; b) pouring the acrylic impact modifier, HL processing aid, external lubricant, composite calcium zinc heat stabilizer, modified toughening agent, antioxidant, light stabilizer, ultraviolet absorber, and recycled powder into the mixer and mixing at a high speed of 950-1000 rpm until the material reaches 125° C.; c) Continue stirring at low speed for 6 to 8 minutes at 125°C and then discharge the material into a cooling mixer; d) When the materials are stirred and cooled to 45-50 degrees in the cooling mixer, they are all released and put into moisture-proof bags for standby use, and the moisture content of the materials is kept below 1%.

4. The composition according to claim 1, It is characterized in that The acrylic ester impact modifier is P335.

5. The composition according to claim 1, It is characterized in that The modified toughening agent is ACM (Acrylate Copolymer Modified) impact toughening agent.

6. The composition according to claim 1, It is characterized in that The external lubricant is oxidized polyethylene wax.

7. A coating process for a door and window profile made of the composition according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Grind the profile surface with a 60 and / or 120 mesh abrasive belt, and then polish it; The treated profile surface is coated with UV paint, wherein the UV paint includes: UV adhesion primer; UV paint; First UV aging resistant topcoat; and Second UV aging resistant topcoat.

8. A coating process for door and window profiles made of the composition according to claim 7, Features: The above coating is applied in six or more layers and dried. Polish the profile surface again before painting, and the amount of paint used for each layer is 10-22 g / m2; The first and second layers of paint should be applied with a brush to ensure uniform coating of the paint and control the dryness at 50%-75%; 3rd-4th layer of UV paint: if it is wood grain surface, only apply the 3rd layer with a brush; if it is full gloss surface, apply the 3rd and 4th layers without a brush, and control the dryness at 75%; The fifth layer of UV topcoat is applied without brush, the paint brightness is 30% ± 3, and the dryness is 75%; The 6th layer of UV topcoat is applied without a brush, the paint gloss is 15% ± 3 and the dryness is 100%.

Citation Information

Patent Citations

  • Paint spraying technology for wood door

    CN106423801A

  • Wide-region high-weathering resistance wood plastic material and preparation method thereof

    CN107383680A

  • Grain fiber wood-like composite material and manufacturing method thereof

    CN113683848A

  • Composition for the production of wood imitations by calendering, injection molding or 3D printing

    DE202015003154U1