Anti-aging PVC cable and preparation method thereof

The ASA particle modified titanium dioxide significantly improves the effect of shielding ultraviolet rays in PVC cables, solves the aging problem of PVC cables, extends the service life, and improves thermal stability and oxidation resistance through optimized formulations.

CN119081313AInactive Publication Date: 2024-12-06GUANGDONG YUEXUN CABLE IND CO LTD

Patent Information

Application Number
CN202411416015.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing PVC cables are prone to aging in light and thermal environments. The traditional UV shielding method cannot effectively prevent UV aging for a long time, resulting in a short service life.

Method used

ASA particles are used to modify silica-coated titanium dioxide to improve its dispersion in PVC, thereby improving the effect of shielding ultraviolet rays and reducing the impact of ultraviolet rays on the PVC matrix.

Benefits of technology

The anti-aging performance of PVC cables is significantly improved, and its service life is extended. The thermal stability and antioxidant ability of the material are enhanced by the combination of preferred components such as calcium and zinc stabilizers, composite antioxidants, etc.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to an anti-aging PVC cable and a preparation method thereof, and belongs to the technical field of PVC cables. The cable material of the anti-aging PVC cable comprises the following components: PVC, a calcium-zinc stabilizer, dioctyl phthalate, cellulose acetate butyrate, calcium carbonate, zinc stearate, a composite antioxidant, zinc stannate and succinic acid. The preparation method comprises the following steps: uniformly mixing cellulose acetate butyrate, zinc stearate and zinc stannate, and grinding to obtain mixed powder; and uniformly mixing the mixed powder, PVC, a calcium-zinc stabilizer, dioctyl phthalate, calcium carbonate, a composite antioxidant and succinic acid, and then carrying out melt blending extrusion and granulation, thereby obtaining the composite material. Titanium dioxide coated with silicon dioxide is modified through ASA particles, the ultraviolet shielding effect of the cable is remarkably improved by improving the dispersity of titanium dioxide in PVC, the influence of ultraviolet rays on the PVC cable can be further relieved, the anti-aging performance of the PVC cable is remarkably improved, and the service life of the PVC cable is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PVC cables and relates to an anti-aging PVC cable and a preparation method thereof. Background Art

[0002] To solve the aging problem of PVC cables, the traditional technical solution is to add ultraviolet shielding materials to the PVC matrix, mainly titanium dioxide, which is widely used in plastics, inks, coatings and cosmetics industries due to its stable physical and chemical properties, high hiding power and whiteness. Coating the surface of titanium dioxide particles with inorganic oxides such as zinc, silicon and aluminum can create a barrier between titanium dioxide and its medium, reduce or inhibit the degradation of the surrounding medium by active oxygen on the surface of titanium dioxide particles, and improve the weather resistance and light resistance of the product.

[0003] Titanium dioxide is added to PVC cables to reduce the effects of ultraviolet rays on the inside of the PVC matrix through physical shielding. Generally, the amount used is large, which has a great impact on the mechanical properties of PVC. Long-term use is prone to surface powdering and orange peel problems. With the progress of the chemical industry, additives that can absorb ultraviolet rays have been developed. These additives can reduce the effects of ultraviolet rays on the PVC matrix. However, the ultraviolet absorbers currently used are easy to migrate from the PVC matrix under light and heat environments and cannot effectively prevent ultraviolet aging in the long term. Therefore, it is necessary to find more effective methods to reduce the effects of ultraviolet rays on the PVC matrix. Summary of the invention

[0004] The object of the present invention is to provide an anti-aging PVC cable and a preparation method thereof. The present invention uses ASA particles to modify silica-coated titanium dioxide, and improves the dispersibility of titanium dioxide in PVC to significantly improve the ultraviolet shielding effect of the cable, thereby further reducing the influence of ultraviolet rays on the PVC cable, significantly improving the anti-aging performance of the cable, and extending its service life.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An anti-aging PVC cable, the anti-aging PVC cable is made of cable material as raw material, sequentially through wire drawing, single wire annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring, and outer sheath extrusion, the cable material comprises the following components by weight:

[0007] PVC 95-100 parts, calcium zinc stabilizer 5-10 parts, dioctyl phthalate 30-40 parts, cellulose acetate butyrate 5-10 parts, calcium carbonate 28-35 parts, zinc stearate 1.2-2.3 parts, composite antioxidant 2-5 parts, zinc stannate 0.6-1.2 parts, succinic acid 0.2-0.4 parts.

[0008] As a preferred technical solution of the present invention, the calcium zinc stabilizer and zinc stearate contain metal salts, which can reduce acid-catalyzed degradation reactions during thermal decomposition, thereby improving the thermal stability of the PVC material.

[0009] As a preferred technical solution of the present invention, when dioctyl phthalate, cellulose acetate butyrate and calcium carbonate are added to the formula, they can act as stabilizers to dilute the HCl acid in the PVC material and slow down the acid-catalyzed degradation reaction, thereby delaying the aging process of the material.

[0010] As a preferred technical solution of the present invention, the carboxylic acid group in succinic acid can form a complex with the cationic stabilizer zinc stearate, and this complex can promote the stability of zinc stearate during thermal decomposition, thereby improving the thermal stability of the PVC material.

[0011] As a preferred technical solution of the present invention, succinic acid can synergize with certain components in the composite antioxidant. The carboxylic acid group in succinic acid and the components in the composite antioxidant may interact through hydrogen bonds, van der Waals forces or coordination bonds to form a complex. This complex can enhance the antioxidant effect of the composite antioxidant and strengthen the ability to inhibit oxidation reactions, thereby improving the anti-aging properties of the material.

[0012] As a preferred technical solution of the present invention, by using ASA-modified silica-coated titanium dioxide, the dispersibility of titanium dioxide in PVC is significantly improved, the ultraviolet shielding effect is enhanced, the influence of ultraviolet rays on the PVC matrix can be further reduced, its anti-aging performance can be significantly improved, and its service life can be extended.

[0013] As a preferred technical solution of the present invention, dioctyl phthalate has good compatibility with polyvinyl chloride and cellulose acetate butyrate, and dioctyl phthalate has good electrical insulation, cold resistance, weather resistance, and volatility resistance, and its addition can improve the stability of the viscosity of the plasticized paste.

[0014] As a preferred technical solution of the present invention, cellulose acetate butyrate has excellent properties such as moisture resistance, UV resistance, cold resistance, flexibility, transparency and electrical insulation, and has good compatibility with resins and high-boiling point plasticizers. Plastics, sheet bases, films and coatings with different properties can be made according to the different butyryl contents. Molding can be performed by extrusion, injection molding, rotational molding, blow molding, etc., and boiling spraying can also be performed. In addition to hydroxyl and acetyl groups, cellulose acetate butyrate molecules also contain butyryl groups, and their properties are related to the contents of the three groups. The carboxyl group of succinic acid can react with the hydroxyl groups in cellulose acetate butyrate and the composite antioxidant, and a dense cross-linking result is formed by the three, which significantly improves the stability of the cable and improves the dispersibility of the composite antioxidant in the system, thereby significantly improving the anti-aging performance of the PVC cable.

[0015] The invention discloses a method for preparing the composite antioxidant, comprising the following steps:

[0016] 1) titanium dioxide and deionized water are placed in a reaction kettle and mixed, sodium silicate solution is added, stirred and mixed, and the pH value is adjusted to obtain a mixed solution;

[0017] 2) adding a dilute sulfuric acid solution to the reactor to adjust the pH value and heating the reactor for reaction, and filtering to obtain a solid;

[0018] 3) washing, drying and grinding the solid matter to obtain composite particles;

[0019] 4) After ultrasonic treatment of the composite particles and toluene, KH-550 is added and stirred and mixed, and the mixture is heated to reflux, washed and dried to obtain modified particles;

[0020] 5) The ASA particles, the modified particles and acetone are stirred and mixed, ultrasonically dispersed and then dried to obtain a composite antioxidant.

[0021] As a preferred technical solution of the present invention, in step 1), the concentration of the sodium silicate solution is 90-95g / L; the dosage ratio of the titanium dioxide, deionized water and the sodium silicate solution is 200g:1L:15-20g; the condition for adjusting the pH value is to adjust the pH to 10-11; and the titanium dioxide is rutile titanium dioxide.

[0022] As a preferred technical solution of the present invention, in step 2), the condition for adjusting the pH value is to use a dilute sulfuric acid solution with a concentration of 185-200 g / L to adjust the pH to 8.6-9.0; the condition for the heating reaction is to heat to 90-95°C and react for 3-4 hours.

[0023] As a preferred technical solution of the present invention, in step 3), the washing condition is to wash until the filtrate is free of sulfate ions; the drying condition is to dry at 115-120°C for 12-13h; and the grinding condition is to grind until it passes through a 20-50 mesh sieve.

[0024] As a preferred technical solution of the present invention, in step 4), the amount ratio of the composite particles, toluene and KH-550 is 6.7g:180mL:6mL; the time of the ultrasonic treatment is 30-45min; the stirring and mixing condition is stirring at 38-40°C for 6-7h; the heating and reflux condition is heating to 85-90°C and reflux for 2-3h; the drying condition is drying at 75-80°C for 12-15h.

[0025] As a preferred technical solution of the present invention, in step 5), the mass ratio of the ASA particles, the modified particles and acetone is 9:4:30; the ultrasonic dispersion time is 4-5 hours; and the drying conditions are 65-70°C and drying for 15-18 hours.

[0026] The invention discloses a method for preparing an anti-aging PVC cable, and the method for preparing the cable material comprises the following steps:

[0027] S1, mixing cellulose acetate butyrate, zinc stearate and zinc stannate uniformly and grinding them to obtain a mixed powder;

[0028] S2, after the mixed powder, PVC, calcium zinc stabilizer, dioctyl phthalate, calcium carbonate, composite antioxidant and succinic acid are uniformly mixed, melt-blended, extruded and granulated to obtain cable material;

[0029] The preparation method of the anti-aging PVC cable comprises the following steps: using cable material as raw material, sequentially performing wire drawing, single-filament annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring and outer sheath extrusion to obtain the cable.

[0030] As a preferred technical solution of the present invention, in step S1, the uniform mixing condition is mixing at a rotation speed of 100-120 r / min for 20-30 min; the grinding time is 4-8 h; and the particle size of the mixed powder is 4-6 μm.

[0031] As a preferred technical solution of the present invention, in step S2, the extrusion conditions are: extrusion at a rotation speed of 150-280 r / min and a temperature of 140-180°C.

[0032] As a preferred technical solution of the present invention, dioctyl phthalate and cellulose acetate butyrate were purchased from Nantong Runfeng Petrochemical Co., Ltd.; ASA particles were purchased from Dongguan Shenghua Plastic Raw Materials Co., Ltd., brand Chimei, model PW-997.

[0033] Beneficial effects of the present invention:

[0034] The present invention uses ASA particles to modify silicon dioxide-coated titanium dioxide, improves the dispersibility of titanium dioxide in PVC, and significantly improves the ultraviolet shielding effect, which can further reduce the impact of ultraviolet rays on the PVC matrix, significantly improve its anti-aging performance, and extend its service life. DETAILED DESCRIPTION

[0035] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0036] Example 1

[0037] An anti-aging PVC cable, the anti-aging PVC cable is made of cable material as raw material, sequentially through wire drawing, single wire annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring, and outer sheath extrusion, the cable material comprises the following components by weight:

[0038] 95 parts of PVC, 5 parts of calcium zinc stabilizer, 30 parts of dioctyl phthalate, 5 parts of cellulose acetate butyrate, 28 parts of calcium carbonate, 1.2 parts of zinc stearate, 2 parts of composite antioxidant, 0.6 parts of zinc stannate, and 0.2 parts of succinic acid.

[0039] The preparation method of the composite antioxidant comprises the following steps:

[0040] 1) titanium dioxide and deionized water are placed in a reaction kettle, mixed, sodium silicate solution is added, stirred and mixed, and the pH value is adjusted to obtain a mixed solution; wherein the concentration of the sodium silicate solution is 90 g / L; the amount ratio of the titanium dioxide, deionized water and sodium silicate solution is 200 g: 1 L: 15 g; the condition for adjusting the pH value is to adjust the pH to 10;

[0041] 2) adding a dilute sulfuric acid solution to the reactor to adjust the pH value and performing a heating reaction, and filtering to obtain a solid; wherein the condition for adjusting the pH value is to use a dilute sulfuric acid solution with a concentration of 185 g / L to adjust the pH to 8.6; and the condition for the heating reaction is to heat to 90° C. and react for 3 hours;

[0042] 3) washing, drying and grinding the solid to obtain composite particles; wherein the washing condition is to wash until the filtrate is free of sulfate ions; the drying condition is to dry at 115° C. for 12 hours; and the grinding condition is to grind until the solid passes through a 20-mesh sieve;

[0043] 4) After ultrasonic treatment of the composite particles and toluene, KH-550 is added and stirred and mixed, and the mixture is heated and refluxed, followed by washing and drying to obtain modified particles; the amount ratio of the composite particles, toluene and KH-550 is 6.7 g: 180 mL: 6 mL; the ultrasonic treatment time is 30 min; the stirring and mixing condition is stirring at 38° C. for 6 h; the heating and reflux condition is heating to 85° C. and reflux for 2 h; the drying condition is drying at 75° C. for 12 h;

[0044] 5) The ASA particles, modified particles and acetone are stirred and mixed, ultrasonically dispersed and then dried to obtain a composite antioxidant; wherein the mass ratio of the ASA particles, modified particles and acetone is 9:4:30; the ultrasonic dispersion time is 4 hours; and the drying condition is 65° C. and drying for 15 hours.

[0045] A method for preparing a cable material comprises the following steps:

[0046] S1. Mix cellulose acetate butyrate, zinc stearate and zinc stannate and grind them to obtain a mixed powder; wherein the mixing conditions are: mixing at a rotation speed of 100 r / min for 20 min; the grinding time is 4 h; and the particle size of the mixed powder is 4 μm;

[0047] S2. Evenly mix the mixed powder, PVC, calcium zinc stabilizer, dioctyl phthalate, calcium carbonate, composite antioxidant and succinic acid, and then perform melt blending, extrusion and granulation to obtain cable material; wherein the extrusion conditions are extrusion at a rotation speed of 150 r / min and a temperature of 140° C.

[0048] Example 2

[0049] An anti-aging PVC cable, the anti-aging PVC cable is made of cable material as raw material, sequentially through wire drawing, single wire annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring, and outer sheath extrusion, the cable material comprises the following components by weight:

[0050] 98 parts of PVC, 7.5 parts of calcium zinc stabilizer, 35 parts of dioctyl phthalate, 8 parts of cellulose acetate butyrate, 32 parts of calcium carbonate, 1.7 parts of zinc stearate, 3.5 parts of composite antioxidant, 0.9 parts of zinc stannate, and 0.3 parts of succinic acid.

[0051] The preparation method of the composite antioxidant comprises the following steps:

[0052] 1) titanium dioxide and deionized water are placed in a reaction kettle, mixed, sodium silicate solution is added, stirred and mixed, and the pH value is adjusted to obtain a mixed solution; wherein the concentration of the sodium silicate solution is 90-95 g / L; the amount ratio of the titanium dioxide, deionized water and sodium silicate solution is 200 g: 1 L: 18 g; the condition for adjusting the pH value is to adjust the pH to 10.5;

[0053] 2) adding a dilute sulfuric acid solution to the reactor to adjust the pH value and performing a heating reaction, and filtering to obtain a solid; wherein the condition for adjusting the pH value is to use a dilute sulfuric acid solution with a concentration of 193 g / L to adjust the pH value to 8.8; and the condition for the heating reaction is to heat to 92.5° C. and react for 3.5 hours;

[0054] 3) washing, drying and grinding the solid to obtain composite particles; wherein the washing condition is washing until the filtrate is free of sulfate ions; the drying condition is drying at 118° C. for 12.5 hours; and the grinding condition is grinding until the solid passes through a 30-mesh sieve;

[0055] 4) After ultrasonic treatment of the composite particles and toluene, KH-550 is added and stirred and mixed, and the mixture is heated and refluxed, followed by washing and drying to obtain modified particles; the amount ratio of the composite particles, toluene and KH-550 is 6.7 g: 180 mL: 6 mL; the ultrasonic treatment time is 38 min; the stirring and mixing condition is stirring at 39° C. for 6.5 h; the heating and reflux condition is heating to 88° C. and refluxing for 2.5 h; the drying condition is drying at 78° C. for 14 h;

[0056] 5) The ASA particles, modified particles and acetone are stirred and mixed, ultrasonically dispersed and then dried to obtain a composite antioxidant; wherein the mass ratio of the ASA particles, modified particles and acetone is 9:4:30; the ultrasonic dispersion time is 4.5 hours; and the drying condition is 68° C. and drying for 17 hours.

[0057] A method for preparing a cable material comprises the following steps:

[0058] S1, mixing cellulose acetate butyrate, zinc stearate and zinc stannate uniformly and grinding them to obtain a mixed powder; wherein the uniform mixing condition is mixing at a rotation speed of 110 r / min for 25 min; the grinding time is 6 h; the particle size of the mixed powder is 5 μm;

[0059] S2. Evenly mix the mixed powder, PVC, calcium zinc stabilizer, dioctyl phthalate, calcium carbonate, composite antioxidant and succinic acid, and then perform melt blending, extrusion and granulation to obtain cable material; wherein the extrusion conditions are extrusion at a rotation speed of 200 r / min and a temperature of 160° C.

[0060] Example 3

[0061] An anti-aging PVC cable, the anti-aging PVC cable is made of cable material as raw material, sequentially through wire drawing, single wire annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring, and outer sheath extrusion, the cable material comprises the following components by weight:

[0062] 100 parts of PVC, 10 parts of calcium zinc stabilizer, 40 parts of dioctyl phthalate, 10 parts of cellulose acetate butyrate, 35 parts of calcium carbonate, 2.3 parts of zinc stearate, 5 parts of composite antioxidant, 1.2 parts of zinc stannate, and 0.4 parts of succinic acid.

[0063] The preparation method of the composite antioxidant comprises the following steps:

[0064] 1) titanium dioxide and deionized water are placed in a reaction kettle, mixed, sodium silicate solution is added, stirred and mixed, and the pH value is adjusted to obtain a mixed solution; wherein the concentration of the sodium silicate solution is 95 g / L; the amount ratio of the titanium dioxide, deionized water and sodium silicate solution is 200 g: 1 L: 20 g; the condition for adjusting the pH value is to adjust the pH to 11;

[0065] 2) adding a dilute sulfuric acid solution to the reactor to adjust the pH value and performing a heating reaction, and filtering to obtain a solid; wherein the condition for adjusting the pH value is to use a dilute sulfuric acid solution with a concentration of 200 g / L to adjust the pH to 9.0; and the condition for the heating reaction is to heat to 95° C. and react for 4 hours;

[0066] 3) washing, drying and grinding the solid to obtain composite particles; wherein the washing condition is to wash until the filtrate is free of sulfate ions; the drying condition is to dry at 120° C. for 13 hours; and the grinding condition is to grind until the solid passes through a 50-mesh sieve;

[0067] 4) After ultrasonic treatment of the composite particles and toluene, KH-550 is added and stirred and mixed, and the mixture is heated and refluxed, followed by washing and drying to obtain modified particles; the amount ratio of the composite particles, toluene and KH-550 is 6.7 g: 180 mL: 6 mL; the ultrasonic treatment time is 45 min; the stirring and mixing condition is stirring at 40° C. for 7 h; the heating and reflux condition is heating to 90° C. and reflux for 3 h; the drying condition is drying at 80° C. for 15 h;

[0068] 5) The ASA particles, modified particles and acetone are stirred and mixed, ultrasonically dispersed and then dried to obtain a composite antioxidant; wherein the mass ratio of the ASA particles, modified particles and acetone is 9:4:30; the ultrasonic dispersion time is 5 hours; and the drying condition is 70° C. and drying for 18 hours.

[0069] A method for preparing a cable material comprises the following steps:

[0070] S1. Mix cellulose acetate butyrate, zinc stearate and zinc stannate and grind them to obtain a mixed powder; wherein the mixing conditions are: mixing at a rotation speed of 120 r / min for 30 min; the grinding time is 8 h; and the particle size of the mixed powder is 6 μm;

[0071] S2. Evenly mix the mixed powder, PVC, calcium zinc stabilizer, dioctyl phthalate, calcium carbonate, composite antioxidant and succinic acid, and then perform melt blending, extrusion and granulation to obtain cable material; wherein the extrusion conditions are extrusion at a rotation speed of 280 r / min and a temperature of 180° C.

[0072] Example 4

[0073] Compared with Example 2, the difference is that the composite antioxidant in Example 4 is 5 parts, and the other components, preparation steps and parameters are the same.

[0074] Example 5

[0075] Compared with Example 2, the difference is that the succinic acid in Example 5 is 0.4 parts, and the other components, preparation steps and parameters are the same.

[0076] Comparative Example 1

[0077] Compared with Example 2, the difference is that Comparative Example 1 does not use ASA particles, and the other components, preparation steps and parameters are the same.

[0078] Comparative Example 2

[0079] Compared with Example 2, the difference lies in the preparation method of the composite antioxidant, and the other components, preparation steps and parameters are the same.

[0080] The preparation method of the composite antioxidant comprises the following steps:

[0081] 1) After ultrasonic treatment of titanium dioxide and toluene passed through a 30-mesh sieve, KH-550 is added and stirred and mixed, and the mixture is washed and dried after heating and reflux to obtain modified particles; the amount ratio of the titanium dioxide, toluene and KH-550 is 6.7 g: 180 mL: 6 mL; the ultrasonic treatment time is 38 min; the stirring and mixing condition is stirring at 39° C. for 6.5 h; the heating and reflux condition is heating to 88° C. and refluxing for 2.5 h; the drying condition is drying at 78° C. for 14 h;

[0082] 2) ASA particles, modified particles and acetone are stirred and mixed, ultrasonically dispersed and then dried to obtain a composite antioxidant; wherein the mass ratio of the ASA particles, modified particles and acetone is 9:4:30; the ultrasonic dispersion time is 4.5 hours; and the drying condition is 68° C. and drying for 17 hours.

[0083] Comparative Example 3

[0084] Compared with Example 2, the difference is that Comparative Example 3 does not use succinic acid, and the other components, preparation steps and parameters are the same.

[0085] Comparative Example 4

[0086] Compared with Example 2, the difference is that Comparative Example 4 does not use cellulose acetate butyrate, and the other components, preparation steps and parameters are the same.

[0087] The cable materials prepared in Examples 1-5 and Comparative Examples 1-4 were subjected to the following tests:

[0088] 1. Tensile strength and elongation at break test: according to GB / T1040.1-2018;

[0089] 2. UV aging test: according to GB / T 16422.3-2014;

[0090] 3. Calculate the retention rate of tensile strength after 50 days of UV radiation according to the following formula;

[0091] Tensile strength retention rate (%) = (tensile strength after 50 days of ultraviolet radiation / initial tensile strength) × 100%;

[0092] The test results are shown in Table 1.

[0093] Table 1

[0094] Tensile strength(MPa) Elongation at break (%) Tensile strength retention rate (%) Example 1 41.5 205 89.4 Example 2 42.7 212 91.7 Example 3 40.9 203 86.7 Example 4 45.2 215 93.3 Example 5 43.4 223 92.1 Comparative Example 1 37.4 175 71.5 Comparative Example 2 34.7 168 66.1 Comparative Example 3 39.8 194 84.8 Comparative Example 4 38.1 151 82.1

[0095] From the test results in Table 1, it can be seen that compared with Comparative Examples 1-4, the anti-aging performance of the cable materials prepared in Examples 1-5 is significantly better than that in Comparative Examples 1-4.

[0096] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. An anti-aging PVC cable, which is made of cable material and sequentially undergoes wire drawing, single-filament annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring, and outer sheath extrusion, characterized in that: The cable material comprises the following components by weight: PVC 95-100 parts, calcium zinc stabilizer 5-10 parts, dioctyl phthalate 30-40 parts, cellulose acetate butyrate 5-10 parts, calcium carbonate 28-35 parts, zinc stearate 1.2-2.3 parts, composite antioxidant 2-5 parts, zinc stannate 0.6-1.2 parts, succinic acid 0.2-0.4 parts.

2. The anti-aging PVC cable according to claim 1, characterized in that: The preparation method of the composite antioxidant comprises the following steps: 1) titanium dioxide and deionized water are placed in a reaction kettle and mixed, sodium silicate solution is added, stirred and mixed, and the pH value is adjusted to obtain a mixed solution; 2) adding a dilute sulfuric acid solution to the reactor to adjust the pH value and heating the reactor for reaction, and filtering to obtain a solid; 3) washing, drying and grinding the solid matter to obtain composite particles; 4) After ultrasonic treatment of the composite particles and toluene, KH-550 is added and stirred and mixed, and the mixture is heated to reflux, washed and dried to obtain modified particles; 5) The ASA particles, the modified particles and acetone are stirred and mixed, ultrasonically dispersed and then dried to obtain a composite antioxidant.

3. The anti-aging PVC cable according to claim 2, characterized in that: In step 1), the concentration of the sodium silicate solution is 90-95 g / L; the usage ratio of the titanium dioxide, deionized water and the sodium silicate solution is 200 g:1 L:15-20 g; and the condition for adjusting the pH value is to adjust the pH to 10-11.

4. The anti-aging PVC cable according to claim 2, characterized in that: In step 2), the pH value is adjusted to 8.6-9.0 using a dilute sulfuric acid solution with a concentration of 185-200 g / L; the heating reaction is heated to 90-95° C. and reacted for 3-4 hours.

5. The anti-aging PVC cable according to claim 2, characterized in that: In step 3), the washing condition is to wash until the filtrate is free of sulfate ions; the drying condition is to dry at 115-120° C. for 12-13 hours; and the grinding condition is to grind until it passes through a 20-50 mesh sieve.

6. The anti-aging PVC cable according to claim 2, characterized in that: In step 4), the amount ratio of the composite particles, toluene and KH-550 is 6.7g:180mL:6mL; the ultrasonic treatment time is 30-45min; the stirring and mixing conditions are stirring at 38-40°C for 6-7h; the heating and reflux conditions are heating to 85-90°C and reflux for 2-3h; the drying conditions are drying at 75-80°C for 12-15h.

7. The anti-aging PVC cable according to claim 2, characterized in that: In step 5), the mass ratio of the ASA particles, the modified particles and acetone is 9:4:30; the ultrasonic dispersion time is 4-5 hours; and the drying conditions are 65-70° C. and 15-18 hours.

8. A method for preparing an anti-aging PVC cable according to any one of claims 1 to 7, characterized in that: The preparation method of the cable material comprises the following steps: S1, mixing cellulose acetate butyrate, zinc stearate and zinc stannate uniformly and grinding them to obtain a mixed powder; S2, after the mixed powder, PVC, calcium zinc stabilizer, dioctyl phthalate, calcium carbonate, composite antioxidant and succinic acid are uniformly mixed, melt-blended, extruded and granulated to obtain cable material; The preparation method of the anti-aging PVC cable comprises the following steps: using cable material as raw material, sequentially performing wire drawing, single-filament annealing, conductor twisting, insulation extrusion, cabling, inner and outer layer extrusion, armoring and outer sheath extrusion to obtain the cable.

9. The method for preparing an anti-aging PVC cable according to claim 8, characterized in that: In step S1, the uniform mixing conditions are: mixing at a rotation speed of 100-120 r / min for 20-30 min; the grinding time is 4-8 h; and the particle size of the mixed powder is 4-6 μm.

10. The method for preparing an anti-aging PVC cable according to claim 8, characterized in that: In step S2, the extrusion conditions are: extrusion at a rotation speed of 150-280 r / min and a temperature of 140-180°C.

Citation Information

Patent Citations

  • Manufacture method for low-voltage electric power cable used for nuclear power station

    CN102347109A

  • Intermediate voltage power cable and production method thereof

    CN107359018A

  • Outdoor ultraviolet-resistant super-weatherable and high temperature-resistant polyvinyl chloride cable material and preparation method thereof

    CN107383696A

  • High-flexibility polyvinyl chloride resin composition and high-flexibility towline cable

    CN107488314A

  • Production method of wear-resistant and tensile flexible cable