Epoxy resin composite material with high glossiness and high toughness and preparation method thereof
The formulation of a high-gloss and high-toughness epoxy resin composite material addresses the challenge of achieving both properties by using specific particle sizes and types of additives, enhancing mechanical and aesthetic qualities.
Patent Information
- Application Number
- CN202411404479.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
AI Technical Summary
Existing epoxy resins struggle to achieve both high gloss and high toughness, limiting their use in high-end materials and building decoration.
A high-gloss and high-toughness epoxy resin composite material is formulated using specific particle sizes and types of porous silica, polybutadiene rubber powder, and modification aids, along with selected curing agents, to enhance interaction and compatibility within the epoxy resin matrix.
The composite material achieves both high gloss and toughness, with improved interaction forces and compatibility, resulting in enhanced mechanical properties and appearance.
Smart Images

Figure BDA0005076152840000021 
Figure BDA0005076152840000071 
Figure BDA0005076152840000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of epoxy resin composite materials, and in particular relates to an epoxy resin composite material with high gloss and high toughness and a preparation method thereof. Background Art
[0002] Epoxy resins, also known as polyepoxides, are a class of reactive prepolymers and polymers containing epoxide groups. Epoxy resins can react with themselves (crosslink) by catalytic homopolymerization, or with a variety of co-reactants, including multifunctional amines, acids (and anhydrides), phenols, alcohols, and mercaptans (sometimes called thiols), which are often referred to as hardeners or curing agents, and the crosslinking reaction is often referred to as curing. Polyepoxides react with themselves or with multifunctional hardeners to form thermosetting polymers, which generally have good mechanical properties, heat resistance, and chemical resistance.
[0003] Epoxy resins are widely used in electronics, electrical components (such as chips on boards), LEDs, high-voltage electrical insulators, paint manufacturing, fiber-reinforced plastic materials, and adhesives for structures and other purposes. However, most of the epoxy resins on the market have only a single excellent toughness and a single outstanding high gloss, so it is extremely easy to limit their use as raw materials for high-end 3C materials or building decoration materials. Previous studies have been conducted on the improvement of the gloss and toughness of epoxy resins and composite materials, but the focus is often on improving a specific performance, and how to significantly improve the toughness of epoxy resins while improving the gloss has not been reported. Therefore, how to provide an epoxy resin composite material with both high gloss and high toughness has become a technical problem that needs to be solved urgently. Summary of the invention
[0004] The purpose of the present invention is to provide an epoxy resin composite material with high gloss and high toughness and a preparation method thereof, which solves the problem in the prior art that it is difficult to achieve epoxy resin composite materials with both high gloss and high toughness.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A high-gloss and high-toughness epoxy resin composite material, the epoxy resin composite material comprises the following raw material components by weight:
[0007]
[0008] Furthermore, the epoxy resin prepolymer has an epoxy equivalent of 0.40-0.55 mol / 100g, a viscosity of 15-120 Pa·s at room temperature, and a number average molecular weight of 500-3000 g / mol.
[0009] As a preferred technical solution of the present invention, the porous silica has a porosity of 90-98%, an average particle size of 40-90 nm, and a density of 0.006-0.01 g / cm 3 .
[0010] As a preferred technical solution of the present invention, the average particle size of the polybutadiene rubber powder is 20-60 nm.
[0011] Furthermore, the polybutadiene rubber powder is subjected to graft modification treatment, the graft modifier is any one of maleic anhydride, styrene and acrylonitrile, and the graft rate is 45-75%.
[0012] As a preferred technical solution of the present invention, the modification aid A includes at least one of isoparaffin, epoxy fatty acid methyl ester, epoxy soybean oil, methyl silicone oil, paraffin, kerosene, white oil, and amino silicone oil.
[0013] Furthermore, the isoparaffin includes C13-14 isoparaffin, CAS number: 93572-05-7.
[0014] As a preferred technical solution of the present invention, the modification aid B includes any one of modified zirconium dioxide and modified aluminum oxide.
[0015] Furthermore, the modified raw materials of the modified zirconium dioxide and modified aluminum oxide are zirconium dioxide and aluminum oxide respectively.
[0016] Furthermore, the average particle size of the modified raw materials is 30-120 nm.
[0017] Furthermore, the preparation method of the modification aid B is:
[0018] A1. Dry the modified raw material under vacuum at controlled temperature to obtain a dried modified raw material for standby use; mix anhydrous ethanol and distilled water evenly to obtain an intermediate liquid A for standby use; mix the coupling agent and anhydrous ethanol evenly and disperse them by ultrasonication to obtain an intermediate liquid B for standby use;
[0019] A2. Evenly mix the dried modified raw material and intermediate liquid A and disperse them by ultrasonic, add intermediate liquid B and reflux in a constant temperature water bath, cool to room temperature after reflux, separate by suction filtration, dry and grind to obtain modified auxiliary agent B.
[0020] Furthermore, the coupling agent in step A1 includes any one of an aluminate coupling agent, a silane coupling agent and a titanate coupling agent.
[0021] Furthermore, the model of the aluminate coupling agent includes DL411, which is purchased from Hubei Maidehao Biotechnology Co., Ltd.; the model of the silane coupling agent includes any one of KH-550, KH-560 and KH-570; the model of the titanate coupling agent includes any one of TC-27 and TC-130, all of which are purchased from Nanjing Tengchuan Technology Co., Ltd.
[0022] Furthermore, in the preparation of intermediate solution A in step A1, the volume ratio of anhydrous ethanol to distilled water is 1:1; in the preparation of intermediate solution B, the amount ratio of the coupling agent to anhydrous ethanol is 0.9-1.1 g:100 mL.
[0023] Furthermore, in step A1, the temperature of the temperature-controlled vacuum drying is 75-80° C. and the time is 3-3.5 hours; and the time of the ultrasonic dispersion is 20-30 minutes.
[0024] Furthermore, in step A2, the usage ratio of the dried modified raw material, intermediate liquid A and intermediate liquid B is 2-2.1 g: 295-305 mL: 95-105 mL.
[0025] Furthermore, in step A2, the ultrasonic dispersion time is 20-30 min; the temperature of the constant temperature water bath is 75-80° C.; and the reflux time is 6-7 h.
[0026] As a preferred technical solution of the present invention, the curing agent A includes any one of trimethylhexamethylene diamine, isophorone diamine and polyether amine.
[0027] As a preferred technical solution of the present invention, the curing agent B is any one of diethyltoluenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone and m-phenylenediamine.
[0028] A method for preparing a high-gloss and high-toughness epoxy resin composite material comprises the following steps:
[0029] (1) mixing epoxy resin prepolymer, porous silica, polybutadiene rubber powder and modification aid A and stirring uniformly to obtain intermediate material A;
[0030] (2) adding modifying agent B, curing agent A and curing agent B to intermediate material A, mixing and stirring evenly to obtain intermediate material B;
[0031] (3) The intermediate material B is first heated under controlled temperature, and then heated under controlled temperature again to obtain a finished epoxy resin composite material.
[0032] As a preferred technical solution of the present invention, the temperature of the temperature-controlled first heating in step (3) is 50-80°C for 10-50 minutes; the temperature of the temperature-controlled second heating is 140-180°C for 50-60 minutes.
[0033] Beneficial effects of the present invention:
[0034] (1) The average particle sizes of the porous silica, polybutadiene rubber powder and modification aid B selected in the present invention are determined through a large number of experimental screenings. Under the average particle size selected in the present invention, they have a very strong interaction force with the epoxy resin prepolymer matrix, can be effectively dispersed evenly in the matrix, and will not reduce the glossiness of the composite material;
[0035] In addition, the present invention compounds curing agent A, curing agent B and porous silica to provide the system with functional group structures such as benzene rings; and compounds porous silica, modification aid A and modification aid B to increase compatibility with the epoxy resin prepolymer matrix and produce stronger interaction; thereby improving the glossiness of the finished epoxy resin composite material.
[0036] (2) The present invention uses polybutadiene rubber powder as the main toughening agent and uses a modified auxiliary agent A to enhance the compatibility of the polybutadiene rubber powder with the epoxy resin prepolymer matrix, and effectively produces a plasticizing effect in the system, thereby greatly increasing the toughness of the finished epoxy resin composite material. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Example 1
[0039] Prepare a modification aid B, wherein the modification aid B includes modified zirconium dioxide; the modification raw material of the modified zirconium dioxide is zirconium dioxide; the average particle size of the modified raw material is 120;
[0040] The preparation methods of the modified zirconium dioxide are:
[0041] A1. Control the temperature of zirconium dioxide at 75°C and vacuum dry for 3 hours to obtain a dried modified raw material, which is set aside; mix anhydrous ethanol and distilled water in a volume ratio of 1:1 to obtain an intermediate liquid A, which is set aside; mix an aluminate coupling agent and anhydrous ethanol in a dosage ratio of 0.9g:100mL and ultrasonically disperse for 25 minutes to obtain an intermediate liquid B, which is set aside;
[0042] The model of the aluminate coupling agent is DL411, purchased from Hubei Maidehao Biotechnology Co., Ltd.;
[0043] A2, the dried modified raw material and intermediate liquid A were mixed evenly and ultrasonically dispersed for 30 minutes, and the intermediate liquid B was added to reflux in a constant temperature water bath at 75°C for 6.5 hours. After the reflux was completed, the modified additive B was obtained by cooling to room temperature, filtering, drying, and grinding.
[0044] The usage ratio of the dried modified raw material, intermediate liquid A and intermediate liquid B is 2.1 g:295 mL:105 mL.
[0045] A modification aid B is prepared, wherein the modification aid B comprises modified alumina. The preparation method of the modified alumina is the same as the preparation method of the modified zirconium dioxide, except that the modified raw material of the modified alumina is alumina, and the average particle size is 30 nm.
[0046] Example 2
[0047] Prepare a modification aid B, wherein the modification aid B includes modified zirconium dioxide; the modification raw material of the modified zirconium dioxide is zirconium dioxide; and the average particle size of the modified raw material is 30 nm;
[0048] The preparation methods of the modified zirconium dioxide are:
[0049] A1. Control the temperature of zirconium dioxide to 80°C and vacuum dry for 3 hours to obtain a dried modified raw material for standby use; mix anhydrous ethanol and distilled water in a volume ratio of 1:1 to obtain an intermediate liquid A for standby use; mix a titanate coupling agent and anhydrous ethanol in a dosage ratio of 1.1 g:100 mL and ultrasonically disperse for 20 minutes to obtain an intermediate liquid B for standby use;
[0050] The model of the silane coupling agent is KH-570;
[0051] A2, the dried modified raw material and intermediate liquid A were mixed evenly and ultrasonically dispersed for 20 minutes, and the intermediate liquid B was added to reflux in a constant temperature water bath at 77.5°C for 6 hours. After the reflux was completed, the modified additive B was obtained by cooling to room temperature, filtering, drying, and grinding.
[0052] The usage ratio of the dried modified raw material, intermediate liquid A and intermediate liquid B is 2.05g:305mL:95mL.
[0053] Prepare a modification aid B, wherein the modification aid B includes modified alumina. The preparation method of the modified alumina is the same as the preparation method of the modified zirconium dioxide, except that the modified raw material of the modified alumina is alumina, and the average particle size is 120 nm. The model of the silane coupling agent is KH-560.
[0054] Example 3
[0055] Prepare a modification aid B, wherein the modification aid B includes modified zirconium dioxide; the modification raw material of the modified zirconium dioxide is zirconium dioxide; and the average particle size of the modified raw material is 80 nm;
[0056] The preparation methods of the modified zirconium dioxide are:
[0057] A1. Control the temperature of zirconium dioxide at 77.5°C and vacuum dry for 3.5 hours to obtain a dried modified raw material for standby use; mix anhydrous ethanol and distilled water at a volume ratio of 1:1 to obtain an intermediate liquid A for standby use; mix a silane coupling agent and anhydrous ethanol at a dosage ratio of 1g:100mL and ultrasonically disperse for 30 minutes to obtain an intermediate liquid B for standby use;
[0058] The titanate coupling agent is TC-2, purchased from Nanjing Tengchuan Technology Co., Ltd.
[0059] A2, the dried modified raw material and the intermediate liquid A were mixed evenly and ultrasonically dispersed for 25 minutes, and the intermediate liquid B was added to reflux in a constant temperature water bath at 80°C for 7 hours. After the reflux was completed, the modified additive B was obtained by cooling to room temperature, filtering, drying and grinding.
[0060] The usage ratio of the dried modified raw material, intermediate liquid A and intermediate liquid B is 2g:300mL:100mL.
[0061] A modification aid B is prepared, wherein the modification aid B includes modified alumina. The preparation method of the modified alumina is the same as the preparation method of the modified zirconium dioxide, except that the modified raw material of the modified alumina is alumina, and the average particle size is 80 nm. The titanate coupling agent is of model TC-130, which is purchased from Nanjing Tengchuan Technology Co., Ltd.
[0062] Example 4
[0063] A high-gloss and high-toughness epoxy resin composite material, the epoxy resin composite material comprises the following raw material components by weight:
[0064]
[0065] The epoxy resin prepolymer has an epoxy equivalent of 0.40 mol / 100 g, a viscosity of 100 Pa·s at room temperature, and a number average molecular weight of 500 g / mol;
[0066] The porous silica has a porosity of 90%, an average particle size of 90 nm, and a density of 0.006 g / cm 3 ;
[0067] The average particle size of the polybutadiene rubber powder is 60 nm, and the powder has been subjected to graft modification treatment, the graft modifier is maleic anhydride, and the graft rate is 45%;
[0068] The modification aid A includes epoxidized soybean oil;
[0069] The modification aid B includes the modified zirconium dioxide obtained in Example 1;
[0070] The curing agent A includes isophorone diamine;
[0071] The curing agent B includes diethyltoluenediamine;
[0072] The method for preparing the high-gloss and high-toughness epoxy resin composite material specifically comprises the following steps:
[0073] (1) mixing epoxy resin prepolymer, porous silica, polybutadiene rubber powder and modification aid A and stirring uniformly to obtain intermediate material A;
[0074] (2) adding modifying agent B, curing agent A and curing agent B to intermediate material A, mixing and stirring evenly to obtain intermediate material B;
[0075] (3) The intermediate material B is heated at 50°C for 50 min, and then heated at 140°C for another 50 min to obtain a finished epoxy resin composite material.
[0076] Example 5
[0077] A high-gloss and high-toughness epoxy resin composite material, the epoxy resin composite material comprises the following raw material components by weight:
[0078]
[0079] The epoxy equivalent of the epoxy resin prepolymer is 0.55 mol / 100g, the viscosity at room temperature is 15 Pa·s, and the number average molecular weight is 1500 g / mol;
[0080] The porous silica has a porosity of 95%, an average particle size of 60 nm, and a density of 0.008 g / cm 3 ;
[0081] The average particle size of the polybutadiene rubber powder is 20 nm, and the powder has been subjected to grafting modification, the grafting modifier is styrene, and the grafting rate is 75%;
[0082] The modification aid A comprises epoxy fatty acid methyl ester;
[0083] The modification aid B includes the modified alumina prepared in Example 3;
[0084] The curing agent A includes trimethyl hexamethylene diamine;
[0085] The curing agent B includes 4,4' diaminodiphenylmethane;
[0086] The method for preparing the high-gloss and high-toughness epoxy resin composite material specifically comprises the following steps:
[0087] (1) mixing epoxy resin prepolymer, porous silica, polybutadiene rubber powder and modification aid A and stirring uniformly to obtain intermediate material A;
[0088] (2) adding modifying agent B, curing agent A and curing agent B to intermediate material A, mixing and stirring evenly to obtain intermediate material B;
[0089] (3) The intermediate material B is heated at 65.5°C for 10 min, and then heated at 160°C for another 55 min to obtain a finished epoxy resin composite material.
[0090] Example 6
[0091] A high-gloss and high-toughness epoxy resin composite material, the epoxy resin composite material comprises the following raw material components by weight:
[0092]
[0093] The epoxy resin prepolymer has an epoxy equivalent of 0.50 mol / 100 g, a viscosity of 120 Pa·s at room temperature, and a number average molecular weight of 3000 g / mol;
[0094] The porous silica has a porosity of 98%, an average particle size of 40 nm, and a density of 0.01 g / cm 3 ;
[0095] The polybutadiene rubber powder has an average particle size of 40 nm and is graft-modified. The graft modifier is acrylonitrile and the graft rate is 60%.
[0096] The modification aid A includes C13-14 isoparaffin;
[0097] The modification aid B includes the modified zirconium dioxide obtained in Example 2;
[0098] The curing agent A comprises polyetheramine;
[0099] The curing agent B includes m-phenylenediamine;
[0100] The method for preparing the high-gloss and high-toughness epoxy resin composite material specifically comprises the following steps:
[0101] (1) mixing epoxy resin prepolymer, porous silica, polybutadiene rubber powder and modification aid A and stirring uniformly to obtain intermediate material A;
[0102] (2) adding modifying agent B, curing agent A and curing agent B to intermediate material A, mixing and stirring evenly to obtain intermediate material B;
[0103] (3) The intermediate material B is heated at 80°C for 30 minutes, and then heated at 180°C for another 60 minutes to obtain a finished epoxy resin composite material.
[0104] Comparative Example 1
[0105] Compared with Example 6, the difference is that in Comparative Example 1, curing agent A is not added, while curing agent B is 31 parts by weight, porous silica is 13 parts by weight, and other operating steps and parameters remain unchanged.
[0106] Comparative Example 2
[0107] Compared with Example 6, the difference is that in Comparative Example 2, curing agent B is not added, while curing agent A is 32 parts by weight, porous silica is 12 parts by weight, and other operating steps and parameters remain unchanged.
[0108] Comparative Example 3
[0109] Compared with Example 6, the difference is that in Comparative Example 3, porous silica is not added, while curing agent A is 23 parts by weight, curing agent B is 21 parts by weight, and the other operating steps and parameters remain unchanged.
[0110] Comparative Example 4
[0111] Compared with Example 6, the difference is that in Comparative Example 4, porous silica is not added, but the modification aid A is 5 parts by weight, the modification aid B is 6 parts by weight, and the other operating steps and parameters remain unchanged.
[0112] Comparative Example 5
[0113] Compared with Example 6, the difference is that in Comparative Example 5, no modifying agent A is added, but the porous silica is 4 parts by weight, the modifying agent B is 7 parts by weight, and the other operating steps and parameters remain unchanged.
[0114] Comparative Example 6
[0115] Compared with Example 6, the difference is that in Example 6, no modifying agent B is added, but the porous silica is 4.5 parts by weight, the modifying agent A is 6.5 parts by weight, and the other operating steps and parameters remain unchanged.
[0116] Comparative Example 7
[0117] Compared with Example 6, the difference is that in Comparative Example 7, no polybutadiene rubber powder is added, and the other operating steps and parameters remain unchanged.
[0118] Comparative Example 8
[0119] Compared with Example 6, the difference is that in Comparative Example 8, no modifying agent A is added, and the other operating steps and parameters remain unchanged.
[0120] Test Case
[0121] (1) Glossiness test: According to GB / T 9754-2007, the finished epoxy resin composite materials prepared in Examples 4 to 6 of the present invention and Comparative Examples 1 to 6 were tested for glossiness; evaluation criteria: glossiness above 90 GU is considered high glossiness, and the results are shown in Table 1;
[0122] (2) Toughness test: According to ASTM D256-10, toughness test was performed on the epoxy resin composite products prepared in Examples 4-6 of the present invention and Comparative Examples 7-8; evaluation criteria: I ZOD impact strength ≥ 25 J / m indicates high toughness. The results are shown in Table 1.
[0123] Table 1
[0124]
[0125]
[0126] It can be seen from the glossiness data in Table 1 that the present invention compounded the curing agent A, the curing agent B and the porous silica, and also compounded the porous silica, the modifying agent A and the modifying agent B, which effectively improved the glossiness of the finished epoxy resin composite material;
[0127] It can be seen from the ZOD impact strength data in Table 1I that the present invention uses polybutadiene rubber powder as the main toughening agent and is supplemented with the modifying agent A, which can greatly increase the toughness of the finished epoxy resin composite material.
[0128] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0129] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A high-gloss and high-toughness epoxy resin composite material, characterized in that: The epoxy resin composite material comprises the following raw materials in parts by weight:
2. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The epoxy equivalent of the epoxy resin prepolymer is 0.40-0.55 mol / 100 g, the viscosity at room temperature is 15-120 Pa·s, and the number average molecular weight is 500-3000 g / mol.
3. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The porous silica has a porosity of 90-98%, an average particle size of 40-90 nm, and a density of 0.006-0.01 g / cm 3 .
4. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The average particle size of the polybutadiene rubber powder is 20-60 nm.
5. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The modification aid A includes at least one of isoparaffin, epoxy fatty acid methyl ester, epoxy soybean oil, methyl silicone oil, paraffin, kerosene, white oil, and amino silicone oil.
6. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The modification aid B includes any one of modified zirconium dioxide and modified aluminum oxide.
7. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The preparation methods of the modified additive B are: A1. Dry the modified raw material under vacuum at controlled temperature to obtain a dried modified raw material for standby use; mix anhydrous ethanol and distilled water evenly to obtain an intermediate liquid A for standby use; mix the coupling agent and anhydrous ethanol evenly and disperse them by ultrasonication to obtain an intermediate liquid B for standby use; A2. Evenly mix the dried modified raw material and intermediate liquid A and disperse them by ultrasonic, add intermediate liquid B and reflux in a constant temperature water bath, cool to room temperature after reflux, separate by suction filtration, dry and grind to obtain modified auxiliary agent B.
8. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The curing agent A includes any one of trimethylhexamethylenediamine, isophoronediamine and polyetheramine.
9. The high-gloss and high-toughness epoxy resin composite material according to claim 1, characterized in that: The curing agent B is any one of diethyltoluenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone and m-phenylenediamine.
10. A method for preparing the high-gloss and high-toughness epoxy resin composite material according to any one of claims 1 to 9, characterized in that: The specific steps include: (1) mixing epoxy resin prepolymer, porous silica, polybutadiene rubber powder and modification aid A and stirring uniformly to obtain intermediate material A; (2) adding modifying agent B, curing agent A and curing agent B to intermediate material A, mixing and stirring evenly to obtain intermediate material B; (3) The intermediate material B is first heated under controlled temperature, and then heated under controlled temperature again to obtain a finished epoxy resin composite material.