Glass fiber bread mold and preparation method thereof

By combining glass fiber with nanoparticles, the problem of cumbersome preparation process and insufficient performance of glass fiber bread molds is solved, the thermal conductivity and compressive strength are improved, and the oil absorption is significantly reduced. It is suitable for baking of oil-containing foods Bake and simplify the process steps.

CN119081356APending Publication Date: 2024-12-06FENGYANG JIASONG NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411406699.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The preparation process of glass fiber bread molds is cumbersome, the product has poor morphology and low strength, and the oil absorption property of glass fiber affects the baking performance, limiting the scope of use.

Method used

Modified glass fibers are prepared by combining glass fibers with nanoparticles (such as nanographene or nanobiomass carbon), combined with epoxy resin, silicone rubber and platinum catalysts, and are prepared by two-stage heating treatment and ultrasonic stirring, simplifying the process and improving Compatibility and dispersion.

Benefits of technology

It improves the thermal conductivity and compressive strength of glass fiber products, significantly reduces oil absorption, simplifies the preparation process, is suitable for baking of oil-containing foods, and the process steps are simplified, without the need for laying and filling resins and subsequent processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005076821160000141
    Figure BDA0005076821160000141
Patent Text Reader

Abstract

The invention relates to a glass fiber bread mold and a preparation method thereof, and belongs to the technical field of glass fiber products, the glass fiber bread mold is prepared from the following raw materials by weight: 30-40 parts of modified glass fiber, 40-60 parts of epoxy resin, 10-20 parts of dimethyl silicone rubber, 10-20 parts of methyl vinyl silicone rubber, 0.01-0.05 part of a platinum catalyst, and 1-2 parts of a vulcanizing agent; wherein the modified glass fiber is prepared from glass fiber and nano particles loaded in pores of the glass fiber, and the nano particles comprise nano biomass charcoal particles. According to the invention, the glass fiber is treated, so that a certain strength of a glass fiber product is maintained, the heat conduction effect of the glass fiber product is improved, the oil absorbency is remarkably reduced, and the modified glass fiber is excellent in compatibility and high in dispersity through combination of the nano-particles and the pretreated glass fiber; the silicone rubber can be better combined with epoxy resin, dimethyl silicone rubber and methyl vinyl silicone rubber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass fiber products, and particularly relates to a glass fiber bread mould and a preparation method thereof. Background Art

[0002] The raw materials for preparing the fiberglass bread mold are glass fiber (referred to as fiberglass) and resin, as well as auxiliary agents and additives that may be required. In the preparation process, after preparing the corresponding proportions of glass fiber, resin and required auxiliary agents, the glass fiber is laid on the mold frame, and the resin is filled on the laid glass fiber and solidified to form the surface layer of the mold. Then, the outer frame and internal structure of the mold are made as needed, and the mold is cut, polished and processed to obtain the required shape and size. However, not only is the preparation process cumbersome, but the prepared fiberglass products also have poor morphology and low strength. The reason is that due to the poor fluidity of the glass fiber, the glass fiber may stay on the surface of the mold when filling the resin, resulting in the exposure of the glass fiber on the surface of the product, showing a rough, spotted appearance, and the oil absorption of the glass fiber will affect the baking performance of the mold, thereby limiting the scope of use of the glass fiber products. Summary of the invention

[0003] The purpose of the present invention is to provide a glass fiber bread mold and a preparation method thereof in order to solve the above problems.

[0004] The present invention achieves the above-mentioned purpose through the following technical solutions:

[0005] The present invention provides a glass fiber bread mold, which is made of the following raw materials by weight: 30-40 parts of modified glass fiber, 40-60 parts of epoxy resin, 10-20 parts of dimethyl silicone rubber, 10-20 parts of methyl vinyl silicone rubber, 0.01-0.05 parts of platinum catalyst, and 1-2 parts of vulcanizing agent;

[0006] The modified glass fiber is made of glass fiber and nanoparticles loaded in the pores of the glass fiber; the nanoparticles are one of nanographene particles and nanobiomass carbon particles, and the preparation process of the glass fiber is as follows:

[0007] Ordinary glass fiber is dispersed in an alkaline solution, stirred ultrasonically, and then mixed with an equal mass of carboxymethyl cellulose after cleaning, and subjected to a two-stage heating treatment. In the first stage, the temperature is raised to 350-400°C and maintained for 0.5-1h, then raised to 1200-1300°C and maintained for 0.5-1h. After natural cooling, it is washed several times with ethanol and deionized water to obtain glass fiber.

[0008] As a further optimization scheme of the present invention, the particle size range of the nanoparticles is 10-100 nm.

[0009] As a further optimization scheme of the present invention, the mass ratio of the glass fiber to the nanoparticles is 1:(0.20-0.30).

[0010] As a further optimization scheme of the present invention, the preparation process of the nano biomass carbon particles is: the biomass carbon is washed with alkaline water and then impregnated with a catalyst; after drying, low-temperature heat treatment and continuous high-temperature heat treatment are sequentially performed in an oxygen-free environment, the treated product is washed with acid water, and the treated biomass carbon is ground into powder.

[0011] As a further optimization scheme of the present invention, the catalyst is ammonium sulfate with a mass fraction of 10wt%.

[0012] As a further optimization scheme of the present invention, the oxygen-free environment is nitrogen or argon; the low-temperature heat treatment temperature is 200-250°C and the treatment time is 30-45min; the continuous high-temperature heat treatment is specifically, treating at a temperature of 700-900°C for 30-45min, and then treating at a temperature of 1000-1500°C for 45-60min; the acid water is a hydrochloric acid aqueous solution with a mass fraction of 10-15wt%.

[0013] As a further optimization scheme of the present invention, particles with a particle size of 45-100 nm in the nanoparticles account for 65-85% of the total mass of the nanoparticles.

[0014] As a further optimization scheme of the present invention, the preparation process of the modified glass fiber is: fully dispersing the nanoparticles in a 10wt% ammonium sulfate catalyst solution; immersing the glass fiber in the catalyst solution, stirring with ultrasound, and then standing to obtain the modified glass fiber after drying.

[0015] The present invention also provides a method for preparing the above-mentioned glass fiber bread mold, comprising the following steps:

[0016] (1) mixing the modified glass fiber and the epoxy resin, and stirring them uniformly to obtain a mixture;

[0017] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir evenly, remove bubbles by vacuum pumping, pour the mixture into a Teflon mold, and cure it under heating for 1-2 hours to obtain a glass fiber bread mold.

[0018] As a further optimization scheme of the present invention, the heating temperature in step (2) is 180-220°C.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention processes the glass fiber to increase the thermal conductivity of the glass fiber product while maintaining a certain strength, and significantly reduces the oil absorption. In addition, by combining nanoparticles and pretreated glass fiber, the modified glass fiber has excellent compatibility and strong dispersibility, and can be better combined with epoxy resin, dimethyl silicone rubber, and methyl vinyl silicone rubber.

[0021] (2) The present invention combines nano-biomass carbon particles with glass fibers, which can significantly reduce the oil absorption of glass fiber products, making them more suitable for baking oil-containing foods such as bread and pizza.

[0022] (3) The present invention selects modified glass fiber as the raw material for glass fiber products, and utilizes the production process of silica gel to produce glass fiber molds. Compared with the traditional glass fiber mold process, the process steps of the present invention are simple, the production cycle is short, and there is no need to lay glass fiber and fill resin. There is basically no need to cut, grind, or perform other processing on the mold. DETAILED DESCRIPTION

[0023] The present application is described in further detail below. It is necessary to point out that the following specific implementation methods are only used to further illustrate the present application and cannot be understood as limiting the scope of protection of the present application. Technicians in this field can make some non-essential improvements and adjustments to the present application based on the above application content.

[0024] 1. Materials

[0025] Unless otherwise specified, the methods used in the present invention are conventional methods known to those skilled in the art, and the reagents and other materials used are commercially available products unless otherwise specified.

[0026] The epoxy resin of the present invention is one of glycidyl ether epoxy resin, linear aliphatic epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, and alicyclic epoxy resin. The epoxy resin in the following embodiments adopts glycidyl ester epoxy resin.

[0027] The vulcanizing agent of the present invention is one of dipentadienyl bis(2-pentadienyl) and tert-butyl perbenzoate. Dipentadienyl bis(2-pentadienyl) is used in the following examples.

[0028] The platinum catalyst of the present invention is purchased from Anhui Aiyota Silicone Oil Co., Ltd.

[0029] The biomass charcoal of the present invention is obtained by washing and drying biomass materials and then carbonizing them at high temperature. The biomass materials include but are not limited to corn stalks, rice husks, peanut shells, bamboos, and trees. The high-temperature carbonization temperature is 300-900° C. The following embodiments of the present invention all use rice husk biomass charcoal.

[0030] 2. Methods

[0031] Example 1

[0032] A glass fiber bread mold provided in this embodiment includes the following raw materials, measured by weight: 50 parts of epoxy resin, 30 parts of modified glass fiber, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.01 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0033] The preparation process of modified glass fiber is:

[0034] (1) ordinary glass fiber is dispersed in a sodium hydroxide aqueous solution with a mass fraction of 73wt%, stirred and ultrasonically treated, and then mixed with carboxymethyl cellulose of equal mass after washing, and subjected to a two-stage heating treatment, wherein the temperature is raised to 350°C and maintained for 1h, and then raised to 1200°C and maintained for 1h, and then naturally cooled and washed with ethanol and deionized water for 3 times to obtain glass fiber;

[0035] (2) The biochar was washed with a 10wt% sodium hydroxide aqueous solution and then impregnated with a 10wt% ammonium sulfate catalyst for 45 minutes; after drying at 50-60°C, it was transferred to a box-type atmosphere furnace and treated at 200°C for 30 minutes in a nitrogen environment. After cooling, the temperature was raised to 700°C for 30 minutes, and then the temperature was raised to 1200°C for 45 minutes. After cooling to room temperature, the treated product was taken out, washed twice with a 15wt% hydrochloric acid aqueous solution, and the treated biochar was ground into powder by a nanomachine to obtain nano biochar particles; the nano biochar particles were treated by density gradient ultracentrifugation to obtain nanoparticles with a particle size of 10-100nm, of which nanoparticles with a particle size range of 45-100nm accounted for 65% of the total;

[0036] (3) The nano-biomass carbon particles are fully dispersed in a 10 wt% ammonium sulfate catalyst solution, and the glass fiber is immersed in the catalyst solution. After ultrasonic stirring, the modified glass fiber is allowed to stand and dried to obtain the modified glass fiber; wherein the mass ratio of the glass fiber to the nano-biomass carbon particles is 1:0.2.

[0037] The preparation method of fiberglass bread mold is as follows:

[0038] (1) mixing the modified glass fiber and the epoxy resin according to a mass ratio, and stirring to obtain a mixture;

[0039] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture in proportion, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat and cure at 200° C. for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0040] Example 2

[0041] A glass fiber bread mold provided in this embodiment is made of the following raw materials by weight: 35 parts of modified glass fiber, 50 parts of epoxy resin, 15 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.01 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0042] The preparation process of modified glass fiber is:

[0043] (1) ordinary glass fiber is dispersed in a sodium hydroxide aqueous solution with a mass fraction of 73wt%, stirred and ultrasonically treated, and then mixed with carboxymethyl cellulose of equal mass after washing, and subjected to a two-stage heating treatment, wherein the temperature is raised to 400°C and maintained for 0.5h, and then raised to 1300°C and maintained for 0.5h, and then naturally cooled and washed with ethanol and deionized water for 3 times to obtain glass fiber;

[0044] (2) The biochar was washed with a 10 wt% sodium hydroxide aqueous solution and then impregnated with a 10 wt% ammonium sulfate catalyst for 45 min; dried at 50-60 ° C and transferred to a box-type atmosphere furnace, treated at 200 ° C for 30 min in a nitrogen environment, cooled, and then heated to 700 ° C for 30 min n , and then heated to 1200°C for 45 minutes, and then taken out after cooling to room temperature, and the treated material was washed twice with a 15wt% hydrochloric acid aqueous solution, and the treated biomass charcoal was ground into powder to obtain nano biomass charcoal particles, and the nano biomass charcoal particles were treated by density gradient ultracentrifugation to obtain nanoparticles with a particle size of 10-100nm, of which nanoparticles with a particle size range of 45-100nm accounted for 70% of the total;

[0045] (3) The nano-biomass carbon particles are fully dispersed in a 10 wt% ammonium sulfate catalyst solution, and the glass fiber is immersed in the catalyst solution. After ultrasonic stirring, the modified glass fiber is allowed to stand and dried to obtain the modified glass fiber; wherein the mass ratio of the glass fiber to the nano-biomass carbon particles is 1:0.2.

[0046] The preparation method of fiberglass bread mold is as follows:

[0047] (1) mixing the modified glass fiber and the epoxy resin, and stirring them uniformly to obtain a mixture;

[0048] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0049] Example 3

[0050] A glass fiber bread mold provided in this embodiment is made of the following raw materials by weight: 40 parts of modified glass fiber, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0051] The preparation process of modified glass fiber is:

[0052] (1) ordinary glass fiber is dispersed in a sodium hydroxide aqueous solution with a mass fraction of 73wt%, stirred and ultrasonically treated, and then mixed with carboxymethyl cellulose of equal mass after washing, and subjected to a two-stage heating treatment, wherein the temperature is raised to 400°C and maintained for 0.5h, and then raised to 1300°C and maintained for 0.5h, and then naturally cooled and washed with ethanol and deionized water for 3 times to obtain glass fiber;

[0053] (2) The biochar was washed with a 10wt% sodium hydroxide aqueous solution and then impregnated with a 10wt% ammonium sulfate catalyst for 45 minutes; after drying at 50-60°C, it was transferred to a box-type atmosphere furnace and treated at 200°C for 30 minutes in a nitrogen environment. After cooling, the temperature was raised to 700°C for 30 minutes, and then the temperature was raised to 1200°C for 45 minutes. After cooling to room temperature, the treated product was taken out, washed twice with a 15wt% hydrochloric acid aqueous solution, and the treated biochar was ground into powder to obtain nano biochar particles. The nano biochar particles were treated by density gradient ultracentrifugation to obtain nanoparticles with a particle size of 10-100nm, of which nanoparticles with a particle size range of 45-100nm accounted for 85% of the total.

[0054] (3) The nano-biomass carbon particles are fully dispersed in a 10wt% ammonium sulfate catalyst solution, and the glass fiber is immersed in the catalyst solution. After ultrasonic stirring, the modified glass fiber is allowed to stand and dried to obtain the modified glass fiber; wherein the mass ratio of the glass fiber to the nano-biomass carbon particles is 1:0.2.

[0055] The preparation method of fiberglass bread mold is as follows:

[0056] (1) mixing the modified glass fiber and the epoxy resin, and stirring them uniformly to obtain a mixture;

[0057] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0058] Example 4

[0059] A glass fiber bread mold provided in this embodiment is made of the following raw materials by weight: 40 parts of modified glass fiber, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0060] The preparation process of modified glass fiber is:

[0061] (1) ordinary glass fiber is dispersed in a sodium hydroxide aqueous solution with a mass fraction of 73wt%, stirred and ultrasonically treated, and then mixed with carboxymethyl cellulose of equal mass after washing, and subjected to a two-stage heating treatment, wherein the temperature is raised to 400°C and maintained for 0.5h, and then raised to 1300°C and maintained for 0.5h, and then naturally cooled and washed with ethanol and deionized water for 3 times to obtain glass fiber;

[0062] (2) The biochar was washed with a 10wt% sodium hydroxide aqueous solution and then impregnated with a 10wt% ammonium sulfate catalyst for 45 minutes; after drying at 50-60°C, it was transferred to a box-type atmosphere furnace and treated at 200°C for 30 minutes in a nitrogen environment. After cooling, the temperature was raised to 700°C for 30 minutes, and then the temperature was raised to 1200°C for 45 minutes. After cooling to room temperature, the treated product was taken out, washed twice with a 15wt% hydrochloric acid aqueous solution, and the treated biochar was ground into powder to obtain nano biochar particles. The nano biochar particles were treated by density gradient ultracentrifugation to obtain nanoparticles with a particle size of 10-100nm, wherein nanoparticles with a particle size range of 45-100nm accounted for 45% of the total.

[0063] (3) The nano-biomass carbon particles are fully dispersed in a 10 wt% ammonium sulfate catalyst solution, and the glass fiber is immersed in the catalyst solution. After ultrasonic stirring, the modified glass fiber is allowed to stand and dried to obtain the modified glass fiber; wherein the mass ratio of the glass fiber to the nano-biomass carbon particles is 1:0.2.

[0064] The preparation method of fiberglass bread mold is as follows:

[0065] (1) mixing the modified glass fiber and the epoxy resin, and stirring them uniformly to obtain a mixture;

[0066] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0067] Comparative Example 1

[0068] The glass fiber mold is made of the following raw materials by weight: 40 parts of ordinary glass fiber, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0069] The preparation method of fiberglass bread mold is as follows:

[0070] (1) mixing ordinary glass fiber and epoxy resin, and stirring to obtain a mixture;

[0071] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0072] Comparative Example 2

[0073] The glass fiber mold is made of the following raw materials by weight: 40 parts of glass fiber, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0074] The preparation process of glass fiber 1 is as follows:

[0075] (1) The biochar was washed with a 10wt% sodium hydroxide aqueous solution and then impregnated with a 10wt% ammonium sulfate catalyst for 45 minutes; after drying at 50-60°C, it was transferred to a box-type atmosphere furnace and treated at 200°C for 30 minutes in a nitrogen environment. After cooling, the temperature was raised to 700°C for 30 minutes, and then the temperature was raised to 1200°C for 45 minutes. After cooling to room temperature, the treated product was taken out, washed twice with a 15wt% hydrochloric acid aqueous solution, and the treated biochar was ground into powder to obtain nano biochar particles. The nano biochar particles were treated by density gradient ultracentrifugation to obtain nanoparticles with a particle size of 10-100nm, wherein nanoparticles with a particle size range of 45-100nm accounted for 85% of the total.

[0076] (2) The nano-biomass carbon particles are fully dispersed in a 10 wt% ammonium sulfate catalyst solution, and ordinary glass fibers are immersed in the catalyst solution. After ultrasonic stirring, the fibers are allowed to stand, and then dried to obtain glass fibers 1; wherein the mass ratio of the glass fibers to the nano-biomass carbon particles is 1:0.2.

[0077] The preparation method of fiberglass bread mold is as follows:

[0078] (1) mixing glass fiber 1 and epoxy resin, and stirring to obtain a mixture;

[0079] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0080] Comparative Example 3

[0081] The glass fiber mold is made of the following raw materials by weight: 40 parts of glass fiber, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0082] The preparation process of glass fiber II is as follows:

[0083] Ordinary glass fiber was dispersed in a sodium hydroxide aqueous solution with a mass fraction of 73wt%, stirred ultrasonically, and mixed with an equal mass of carboxymethyl cellulose after cleaning. A two-stage heating treatment was performed. In the first stage, the temperature was raised to 400°C and maintained for 0.5h, then raised to 1300°C and maintained for 0.5h. After natural cooling, it was washed three times with ethanol and deionized water to obtain glass fiber II.

[0084] The preparation method of fiberglass bread mold is as follows:

[0085] (1) mixing glass fiber 2 with epoxy resin and stirring to obtain a mixture;

[0086] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0087] Comparative Example 4

[0088] The glass fiber mold is made of the following raw materials by weight: 40 parts of glass fiber 3, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0089] The preparation process of glass fiber 3 is:

[0090] (1) ordinary glass fiber is dispersed in an alkaline solution, stirred with ultrasound, washed and mixed with carboxymethyl cellulose of equal mass, and subjected to a two-stage heating treatment, wherein the temperature is raised to 400°C and maintained for 0.5 h, then raised to 1300°C and maintained for 0.5 h, and then naturally cooled and washed with ethanol and deionized water for 3 times to obtain glass fiber;

[0091] (2) The biochar particles are ground into powder, fully dispersed in a 10 wt% ammonium sulfate catalyst solution, glass fibers are immersed in the catalyst solution, ultrasonically stirred and allowed to stand, and then dried to obtain modified glass fibers; wherein the mass ratio of the glass fibers to the biochar particles is 1:0.2.

[0092] The preparation method of fiberglass bread mold is as follows:

[0093] (1) mixing glass fiber 3 with epoxy resin, and stirring to obtain a mixture;

[0094] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0095] Comparative Example 5

[0096] The glass fiber mold is made of the following raw materials by weight: 40 parts of glass fiber tetrachloride, 60 parts of epoxy resin, 20 parts of dimethyl silicone rubber, 20 parts of methyl vinyl silicone rubber, 0.02 parts of platinum catalyst, and 1 part of vulcanizing agent;

[0097] The preparation process of glass fiber 4 is:

[0098] (1) ordinary glass fiber is dispersed in a sodium hydroxide aqueous solution with a mass fraction of 73wt%, stirred and ultrasonically treated, and then mixed with carboxymethyl cellulose of equal mass after washing, and subjected to a two-stage heating treatment, wherein the temperature is raised to 400°C and maintained for 0.5h, and then raised to 1300°C and maintained for 0.5h, and then naturally cooled and washed with ethanol and deionized water for 3 times to obtain glass fiber;

[0099] (2) Nano-graphene particles (nano-graphene particles are treated by density gradient ultracentrifugation to obtain nano-particles with a particle size of 10-100 nm, wherein nano-particles with a particle size range of 45-100 nm account for 85% of the total) are fully dispersed in a 10 wt% ammonium sulfate catalyst solution, glass fibers are immersed in the catalyst solution, ultrasonically stirred and allowed to stand, and then dried to obtain modified glass fibers; wherein the mass ratio of glass fibers to nano-biomass carbon particles is 1:0.2.

[0100] The preparation method of fiberglass bread mold is as follows:

[0101] (1) mixing glass fiber 4 and epoxy resin, and stirring to obtain a mixture;

[0102] (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir at a rate of 1000 rpm / min, stir for 10 min, and after stirring evenly, evacuate to 200 Pa to expel the bubbles therein, pour it into a Teflon mold, heat at 200° C. and cure for 1 h, and obtain a glass fiber bread mold after natural cooling.

[0103] 3. Test Verification

[0104] The glass fiber products prepared in Examples 1-4 and Comparative Examples 1-5 were used as test samples to conduct the following tests:

[0105] Thermal conductivity: The thermal conductivity of each sample was measured using a NETZSCH LFA427 laser thermal conductivity meter, and the average value was taken after 5 measurements.

[0106] Compressive strength: The compressive strength of each sample was measured using a WDS series universal testing machine, and the average value was taken after 5 measurements.

[0107] Oil permeability: Soak each test sample in peanut oil at 100°C for 30 minutes, remove the oil on the surface of the test sample, and test the mass increase rate before and after.

[0108] The test results are recorded in the following table:

[0109]

[0110] It can be seen from Examples 1-4 and Comparative Example 1 that the present invention increases the thermal conductivity of glass fiber products while maintaining a certain strength by treating the glass fiber, and significantly reduces the oil absorption, and through the combination of nanoparticles and pretreated glass fiber, the modified glass fiber has excellent compatibility and strong dispersibility, and can be better combined with epoxy resin and dimethyl silicone rubber and methyl vinyl silicone rubber. It was also found in the study that nanoparticles in different particle size ranges have a certain effect on the oil absorption of glass fiber products.

[0111] It can be seen from Examples 1-4 and Comparative Example 2 that when the glass fiber is not pretreated, its compressive strength is significantly reduced and its oil absorption is significantly increased. It is speculated that this may be because the ordinary glass fiber has poor binding properties with the nanoparticles, resulting in its performance not being improved. It can be seen from Comparative Example 3 that after pretreatment, the glass fiber is used as a raw material for glass fiber products, which will lead to a decrease in thermal conductivity and compressive strength of the glass fiber products, and will not affect the oil absorption of the glass fiber products.

[0112] It can be seen from Examples 1-4 and Comparative Examples 4-5 that if the biochar is not treated, its dispersibility and compatibility are poor, which will lead to reduced performance of glass fiber products and affect oil absorption. When the nanoparticles are graphene, their compressive strength is the same as that of nano-biomass carbon particles, and their thermal conductivity is even better than that of glass fiber products using nano-biomass carbon particles, but their oil absorption is high and they are not suitable for food molds such as bread.

[0113] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A fiberglass bread mold, characterized in that: The following raw materials are used in parts by weight: 30-40 parts of modified glass fiber, 40-60 parts of epoxy resin, 10-20 parts of dimethyl silicone rubber, 10-20 parts of methyl vinyl silicone rubber, 0.01-0.05 parts of platinum catalyst, and 1-2 parts of vulcanizing agent; The modified glass fiber is made of glass fiber and nanoparticles loaded in the pores of the glass fiber; the nanoparticles are nano biomass carbon particles, and the preparation process of the glass fiber is as follows: Ordinary glass fiber is dispersed in an alkaline solution, stirred ultrasonically, and then mixed with an equal mass of carboxymethyl cellulose after cleaning, and subjected to a two-stage heating treatment. In the first stage, the temperature is raised to 350-400°C and maintained for 0.5-1h, then raised to 1200-1300°C and maintained for 0.5-1h. After natural cooling, it is washed several times with ethanol and deionized water to obtain glass fiber.

2. A glass fiber bread mold according to claim 1, characterized in that: The particle size of the nanoparticles ranges from 10 to 100 nm.

3. A glass fiber bread mold according to claim 2, characterized in that: The mass ratio of the glass fiber to the nanoparticles is 1:(0.20-0.30).

4. A glass fiber bread mold according to claim 1, characterized in that: The preparation process of the nano biomass carbon particles is as follows: washing the biomass carbon with alkaline water and then impregnating it with a catalyst; After drying, low-temperature heat treatment and continuous high-temperature heat treatment are sequentially performed in an oxygen-free environment, the treated product is washed with acid water, and the treated biochar is ground into powder.

5. A glass fiber bread mold according to claim 4, characterized in that: The catalyst is ammonium sulfate with a mass fraction of 10wt%.

6. A glass fiber bread mold according to claim 5, characterized in that: The oxygen-free environment is nitrogen or argon; the low-temperature heat treatment temperature is 200-250°C and the treatment time is 30-45 minutes; the continuous high-temperature heat treatment is specifically, treating at a temperature of 700-900°C for 30-45 minutes, and then treating at a temperature of 1000-1500°C for 45-60 minutes; the acid water is a hydrochloric acid aqueous solution with a mass fraction of 10-15wt%.

7. The fiberglass bread mold according to claim 1, characterized in that: In the nanoparticles, particles with a particle size of 45-100 nm account for 65-85% of the total mass of the nanoparticles.

8. The fiberglass bread mold according to claim 1, characterized in that: The preparation process of the modified glass fiber is as follows: fully dispersing nanoparticles in a 10wt% ammonium sulfate catalyst solution; immersing glass fibers in the catalyst solution, stirring with ultrasound, and then standing to obtain the modified glass fibers after drying.

9. A method for preparing a glass fiber bread mold as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: (1) mixing the modified glass fiber and the epoxy resin, and stirring them uniformly to obtain a mixture; (2) Add dimethyl silicone rubber, methyl vinyl silicone rubber, platinum catalyst and vulcanizing agent to the mixture, stir evenly, remove bubbles by vacuum pumping, pour the mixture into a Teflon mold, and cure it under heating for 1-2 hours to obtain a glass fiber bread mold.

10. The method for preparing a glass fiber bread mold according to claim 9, characterized in that: The heating temperature in step (2) is 180-220°C.