Flame-retardant heat-conducting insulating silicone rubber and preparation method thereof
By using vinyl-terminated polysiloxane, hydrogen-containing silicone oil and other components in thermally conductive silicone rubber, combined with specific process processing, the problem of reducing insulation caused by improved thermal conductivity and flame retardancy is solved, and thermal conductivity is achieved , good balance of flame retardancy and insulation, meet the needs of high-performance heating components.
Patent Information
- Application Number
- CN202411202590.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
When existing thermally conductive silicone rubber improves thermal conductivity and flame retardancy, it usually leads to a decrease in insulation, making it difficult to find a balance between the two, and cannot meet the demand for high insulation and flame retardancy of heating elements.
Flame-retardant thermally insulated silicone rubber is prepared by a combination of vinyl-terminated polysiloxane, hydrogen-containing silicone oil, aluminum hydroxide, hydrotalcite, inhibitor and platinum catalyst through specific stirring and vacuum treatment processes to ensure that it remains thermally conductive It has good insulation properties and flame retardancy.
A good balance of thermal conductivity, flame retardancy and insulation is achieved, ensuring that after soaking in pure water for 100 hours, the volume resistivity and breakdown voltage resistance can still be maintained at a high level, meeting the needs of high-performance heating elements.
Smart Images

Figure BDA0005018182270000021 
Figure BDA0005018182270000022 
Figure BDA0005018182270000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermally conductive adhesives, and in particular to a flame-retardant thermally conductive insulating silicone rubber and a preparation method thereof. Background Art
[0002] With the continuous improvement of the performance of electronic equipment, the power density of heating elements continues to increase, resulting in more and more heat generated, which not only affects the working efficiency of the corresponding equipment, but also greatly shortens its service life. Thermal conductive silicone rubber is a thermal conductive filling material made of silicone polymer as the base material, with auxiliary materials such as thermal conductive fillers added and made through a specific process. The main function of this type of material is interfacial heat conduction; the liquid rubber can fill the gaps on the contact surface, and can complete the heat transfer between the heating device and the heat dissipation device. After solidifying into a rubber block, it also plays the role of insulation, shock absorption, sealing, etc. It is easy to use and has a wide range of applications. It is widely used in the field of electrical and electronic equipment.
[0003] At present, in order to better meet the needs of heating elements, thermally conductive silicone rubber is required to have high insulation, good flame retardancy and excellent breakdown resistance. The improvement of thermal conductivity and flame retardancy is usually achieved by increasing the amount of filler, but the increase of filler will lead to a decrease in the insulation of silicone rubber. Therefore, the field needs to develop a flame-retardant thermally conductive insulating material that has good insulation while ensuring thermal conductivity and flame retardancy, so as to improve the deficiencies of the existing technology and promote the development of the industry. Summary of the invention
[0004] Based on the above description, the present invention provides a flame retardant thermally conductive insulating silicone rubber and a preparation method thereof to solve the technical problem in the prior art that the thermal conductivity and flame retardancy of the thermally conductive silicone rubber are improved while the insulation is reduced.
[0005] The technical solution of the present invention to solve the above technical problems is as follows:
[0006] In a first aspect, the present invention provides a flame retardant, thermally conductive, insulating silicone rubber, comprising: components added in the following weight parts:
[0007]
[0008] The structural formula of the vinyl-terminated polysiloxane is shown in formula (I):
[0009]
[0010] In formula (I), R1 represents a methyl group or a phenyl group; and n is an integer.
[0011] Based on the above technical solution, the present invention can also be improved as follows.
[0012] Furthermore, the hydrogen-containing silicone oil is a methyl-terminated side hydrogen-containing silicone oil, a silicon-hydrogen bond-terminated side hydrogen-containing silicone oil, or a combination of a side hydrogen-containing silicone oil without silicon-hydrogen bonds and a methyl-terminated side hydrogen-containing silicone oil.
[0013] Furthermore, the hydrogen content in the hydrogen-containing silicone oil is 0.1-0.6 wt %.
[0014] Furthermore, the particle size D50 of the aluminum hydroxide is in the range of 15 to 25 μm, and the content of Na+ is ≤0.05%.
[0015] Furthermore, the particle size D50 of the hydrotalcite is in the range of 0.4 to 1.5 μm, and the conductivity is less than 10 μs / cm.
[0016] Furthermore, the inhibitor is ethynyl cyclohexanol, cyclic vinyl siloxane, tetravinyltetramethylcyclotetrasiloxane or benzotriazole.
[0017] Furthermore, the platinum catalyst is platinum black, platinum chloride, a complex of chloroplatinic acid and a monohydric alcohol, a complex of chloroplatinic acid and an olefin, a chelate of platinum vinylsiloxane or platinum acetoacetate.
[0018] In a second aspect, the present invention further provides a method for preparing the flame-retardant, thermally conductive, insulating silicone rubber according to the first aspect, comprising:
[0019] S1. Add vinyl-terminated polysiloxane and aluminum hydroxide into a planetary stirring kettle, and evacuate the kettle while stirring at 120°C;
[0020] S2. Lower the material temperature to 80°C, add hydrogen-containing silicone oil and hydrotalcite, and evacuate the material while stirring at 80°C;
[0021] S3, lower the material temperature to 40°C, add an inhibitor, and evacuate while stirring while keeping the material temperature below 40°C;
[0022] S4. Add platinum catalyst, keep the material temperature not exceeding 40°C, stir and evacuate at the same time, and finally apply the glue liquid to device potting or tablet molding to obtain flame-retardant, thermally conductive and insulating silicone rubber.
[0023] Based on the above technical solution, the present invention can also be improved as follows.
[0024] Furthermore, in steps S1 and S2, the stirring time of vacuuming while stirring is 60 minutes, and the vacuum pressure is maintained at -0.098 MPa.
[0025] Compared with the prior art, the technical solution of this application has the following beneficial technical effects:
[0026] The flame retardant, heat-conducting, insulating silicone rubber provided by the present invention comprises the following components added in parts by weight:
[0027]
[0028]
[0029] Compared with the prior art, the flame-retardant thermally conductive insulating silicone rubber provided by the present invention has good thermal conductivity, flame retardancy, and good volume resistivity and breakdown voltage resistance (dielectric strength), and the volume resistivity and breakdown voltage resistance after being immersed in pure water for 100 hours can still be maintained within a good range, that is, it has good thermal conductivity and flame retardancy as well as good insulation. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present application, the embodiments of the present invention are further described in detail below in conjunction with examples. The following examples are used to illustrate the present invention but cannot be used to limit the scope of the present invention.
[0031] It should be noted that:
[0032] In the present invention, parts are by weight unless otherwise specified.
[0033] In the present invention, room temperature refers to a temperature of 25°C, and the viscosity values are all measured at 25°C.
[0034] The thermal conductivity was tested using a TPS500 thermal constant analyzer from Hot Disk of Sweden.
[0035] The dielectric strength was tested using a BDJC-100KV voltage breakdown tester.
[0036] The volume resistivity was tested using a ZC36 high insulation resistance tester.
[0037] The flame retardancy level is tested using a vertical burning test machine.
[0038] In order to make the thermally conductive silicone rubber have good thermal conductivity and flame retardancy as well as good insulation, the present invention provides a flame retardant thermally conductive insulating silicone rubber, comprising: components added in the following weight parts:
[0039]
[0040]
[0041] The structural formula of the vinyl-terminated polysiloxane is shown in formula (I):
[0042]
[0043] In formula (I), R1 represents a methyl group or a phenyl group; and n is an integer.
[0044] Preferably, the hydrogen-containing silicone oil is a methyl-terminated side hydrogen-containing silicone oil, a silicon-hydrogen bond-terminated side hydrogen-containing silicone oil, or a combination of a side hydrogen-containing silicone oil without silicon-hydrogen bonds and a methyl-terminated side hydrogen-containing silicone oil. The selection can be made according to actual needs and is not specifically limited here.
[0045] Preferably, the hydrogen content in the hydrogen-containing silicone oil is 0.1-0.6 wt %. Preferably, the particle size D50 of the aluminum hydroxide is in the range of 15-25 μm, and the content of Na+ is ≤0.05%.
[0046] Preferably, the particle size D50 of the hydrotalcite is in the range of 0.4 to 1.5 μm, and the conductivity is less than 10 μs / cm.
[0047] Preferably, the inhibitor is ethynyl cyclohexanol, cyclic vinyl siloxane, tetravinyltetramethylcyclotetrasiloxane or benzotriazole, which can be selected according to actual needs and is not specifically limited here.
[0048] Preferably, the platinum catalyst is platinum black, platinum chloride, a complex of chloroplatinic acid and a monohydric alcohol, a complex of chloroplatinic acid and an olefin, a chelate of platinum vinylsiloxane, or platinum acetoacetate. The catalyst can be selected according to actual needs and is not specifically limited here.
[0049] The present invention is further described below in conjunction with specific embodiments. The specific embodiments are for further describing the present invention in detail, but are not intended to limit the protection scope of the present invention.
[0050] Example 1
[0051] This embodiment provides a flame retardant, thermally conductive, insulating silicone rubber and a preparation method thereof.
[0052] A flame retardant, heat-conducting, insulating silicone rubber, comprising: ingredients added in the following weight proportions:
[0053]
[0054] The corresponding preparation method is as follows:
[0055] Step S1: 100 parts of a vinyl-terminated polysiloxane having a structure of formula (I) (viscosity of about 100 mPa·s, vinyl content of 1.0%, R1 being methyl) and 220 parts of aluminum hydroxide (particle size D50 of 20 μm, Na+ content of 0.03%) were placed in a planetary stirring reactor, and vacuumed (-0.098 MPa) at 120° C. for 60 min while stirring;
[0056] Step S2: the material temperature was lowered to 80°C, 15 parts of terminal hydrogen-containing silicone oil (side groups do not contain silicon-hydrogen bonds, and the hydrogen content is 0.1%) and 4 parts of terminal methyl side hydrogen-containing silicone oil (hydrogen content is 0.6%), and 20 parts of hydrotalcite (particle size D50 is 0.5 μm, conductivity is 5.78 μs / cm) were added, and vacuum (-0.098 MPa) was evacuated at 80°C for 60 min while stirring;
[0057] Step S3: lower the material temperature to 40°C, add 0.025 parts of inhibitor ethynylcyclohexanol, and stir while vacuuming for 20 minutes (keeping the material temperature ≤40°C during the process);
[0058] Step S4: Finally, add 1.2 parts of platinum catalyst (the concentration of Pt in the catalyst is 3000ppm), stir and vacuum for 20 minutes (keeping the material temperature ≤40°C during the process), then shape the rubber hydraulic sheet, and bake at 80°C for 20 minutes to form thin sheets with a thickness of 2mm and 3mm and a rubber block with a thickness of 2cm.
[0059] The initial volume resistivity, dielectric strength (2 mm thin sheet), flame retardancy (3 mm thin sheet) and thermal conductivity (2 cm thick rubber block) of the rubber block obtained in Example 1 were tested, as well as the volume resistivity and dielectric strength of the thin sheet after being immersed in pure water for 100 hours. The results are shown in Table 1.
[0060] Example 2
[0061] This embodiment provides a flame retardant, thermally conductive, insulating silicone rubber and a preparation method thereof.
[0062] A flame retardant, heat-conducting, insulating silicone rubber, comprising: ingredients added in the following weight proportions:
[0063]
[0064] The corresponding preparation method is as follows:
[0065] Step S1: 100 parts of a vinyl-terminated polysiloxane having a structure of formula (I) (viscosity of about 100 mPa·s, vinyl content of 1.0%, R1 being methyl) and 210 parts of aluminum hydroxide (particle size D50 of 20 μm, Na+ content of 0.03%) were placed in a planetary stirring reactor, and vacuumed (-0.098 MPa) at 120° C. for 60 min while stirring;
[0066] Step S2: the material temperature was lowered to 80° C., 13 parts of end-side hydrogen-containing silicone oil (hydrogen content of 0.3%) capped with silicon-hydrogen bonds and 16 parts of hydrotalcite (particle size D50 of 0.5 μm, conductivity of 5.78 μs / cm) were added, and the mixture was stirred at 80° C. while evacuating the mixture (-0.098 MPa) for 60 min;
[0067] Step S3: lower the material temperature to 40°C, add 0.025 parts of inhibitor ethynylcyclohexanol, and stir while vacuuming for 20 minutes (keeping the material temperature ≤40°C during the process);
[0068] Step S4: Finally, add 1.2 parts of platinum catalyst (the concentration of Pt in the catalyst is 3000ppm), stir and vacuum for 20 minutes (keeping the material temperature ≤40°C during the process), then shape the rubber hydraulic sheet, and bake at 80°C for 20 minutes to form thin sheets with a thickness of 2mm and 3mm and a rubber block with a thickness of 2cm.
[0069] The initial volume resistivity, dielectric strength (2 mm thin sheet), flame retardancy (3 mm thin sheet) and thermal conductivity (2 cm thick rubber block) of the rubber block obtained in Example 2 were tested, as well as the volume resistivity and dielectric strength of the thin sheet after being immersed in pure water for 100 hours. The results are shown in Table 1.
[0070] Comparative Example 1
[0071] Compared with the above-mentioned Example 1, the difference of this comparative example is that the aluminum hydroxide (particle size D50 is 20 μm, Na+ content is 0.03%) in Example 1 is replaced by aluminum hydroxide (particle size D50 is 20 μm, Na+ content is 0.1%), and the remaining materials and preparation methods are the same as those in Example 1.
[0072] Comparative Example 2
[0073] Compared with the above-mentioned Example 1, the difference of this comparative example is that the hydrotalcite in Example 1 (particle size D50 is 0.5 μm, conductivity 5.78 μs / cm) is replaced by hydrotalcite (particle size D50 is 0.5 μm, conductivity 14.36 μs / cm), and the remaining materials and preparation methods are the same as those in Example 1.
[0074] Comparative Example 3
[0075] Compared with the above-mentioned Example 1, the difference of this comparative example is that: in Example 1, the step S1 of stirring and vacuuming (-0.098 MPa) at 80°C for 60 min is replaced by stirring for 60 min; the step S2 of stirring and vacuuming (-0.098 MPa) at 80°C for 60 min is replaced by stirring for 60 min, and the remaining materials and preparation methods are the same as those in Example 1.
[0076] The silicone rubber obtained in the above Examples 1 and 2 and Comparative Examples 1 to 3 was tested for volume resistivity, dielectric strength (2 mm thin sheet), flame retardancy (3 mm thin sheet) and thermal conductivity (2 cm thick rubber block), as well as volume resistivity and dielectric strength after the thin sheet was immersed in pure water for 100 hours.
[0077] The test results are shown in Table 1:
[0078] Table 1 Test results of examples and comparative examples
[0079]
[0080] From the above table, it can be seen that the silicone rubber compositions of Example 1 and Example 2 have good thermal conductivity, flame retardancy, and good volume resistivity and breakdown voltage resistance (dielectric strength), and although the volume resistivity and breakdown voltage resistance decrease after immersion in pure water for 100 hours, they can still be maintained within a good range.
[0081] The specifications of the aluminum hydroxide in Comparative Example 1 do not meet the specification requirements of the aluminum hydroxide of the present invention (the corresponding requirements for the ion content of aluminum hydroxide in the present invention can maintain its related electrical properties such as breakdown voltage resistance), the specifications of the hydrotalcite in Comparative Example 2 do not meet the specification requirements of the hydrotalcite of the present invention (the electrical conductivity of the hydrotalcite in the present invention can also affect related electrical properties such as withstand voltage), and the preparation method in Comparative Example 3 is different from that in Example 1 of the present application. The volume resistivity and breakdown voltage resistance of the silicone rubber compositions in these three comparative examples are significantly reduced after being immersed in pure water for 100 hours.
[0082] Therefore, the method for preparing the flame-retardant thermally conductive insulating silicone rubber provided by the present invention and the corresponding flame-retardant thermally conductive insulating silicone rubber prepared have good thermal conductivity, flame retardancy, and good volume resistivity and breakdown voltage resistance (dielectric strength), and the volume resistivity and breakdown voltage resistance after immersion in pure water for 100 hours can still be maintained within a good range, that is, while having good thermal conductivity and flame retardancy, it also has good insulation.
[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A flame retardant, thermally conductive, insulating silicone rubber, characterized in that: The composition includes the following components in parts by weight: 100 parts of vinyl terminated polysiloxane; The ratio of the molar amount of silicon-hydrogen bonds of the hydrogen-containing silicone oil to the molar amount of the vinyl groups in the vinyl-terminated polysiloxane is 0.9 to 1.5; 200-250 parts of aluminum hydroxide; Inhibitor 0.02-0.1 part; The platinum catalyst is based on the total weight of the vinyl-terminated polysiloxane, and the amount of the platinum catalyst is 5 to 50 ppm in terms of platinum (Pt); The hydrotalcite is based on the total weight of the vinyl-terminated polysiloxane, and the weight of the hydrotalcite is 2 to 20% of the total weight of the vinyl-terminated polysiloxane; The structural formula of the vinyl-terminated polysiloxane is shown in formula (I): In formula (I), R1 represents a methyl group or a phenyl group; and n is an integer.
2. The flame retardant, thermally conductive, insulating silicone rubber according to claim 1, characterized in that: The hydrogen-containing silicone oil is a methyl-terminated side hydrogen-containing silicone oil, a silicon-hydrogen bond-terminated side hydrogen-containing silicone oil, or a combination of a side hydrogen-containing silicone oil without silicon-hydrogen bonds and a methyl-terminated side hydrogen-containing silicone oil.
3. The flame retardant, thermally conductive, insulating silicone rubber according to claim 2, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 0.1-0.6 wt %.
4. The flame retardant, thermally conductive, insulating silicone rubber according to claim 1, characterized in that: The particle size D50 of the aluminum hydroxide is in the range of 15 to 25 μm, and the content of Na+ is ≤0.05%.
5. The flame retardant, thermally conductive, insulating silicone rubber according to claim 1, characterized in that: The particle size D50 of the hydrotalcite is in the range of 0.4 to 1.5 μm, and the conductivity is less than 10 μs / cm.
6. The flame retardant, thermally conductive, insulating silicone rubber according to claim 1, characterized in that: The inhibitor is ethynylcyclohexanol, cyclic vinylsiloxane, tetravinyltetramethylcyclotetrasiloxane or benzotriazole.
7. The flame retardant, thermally conductive, insulating silicone rubber according to claim 1, characterized in that: The platinum catalyst is platinum black, platinum chloride, a complex of chloroplatinic acid and monohydric alcohol, a complex of chloroplatinic acid and olefins, a chelate of platinum vinylsiloxane or platinum acetoacetate.
8. A method for preparing the flame-retardant, thermally conductive, insulating silicone rubber according to any one of claims 1 to 7, characterized in that: include: S1. Add vinyl-terminated polysiloxane and aluminum hydroxide into a planetary stirring kettle, and evacuate the kettle while stirring at 120°C; S2. Lower the material temperature to 80°C, add hydrogenated silicone oil and hydrotalcite, and evacuate the material while stirring at 80°C; S3, lower the material temperature to 40°C, add the inhibitor, and evacuate while stirring while keeping the material temperature below 40°C; S4. Add platinum catalyst, keep the material temperature not exceeding 40°C, stir and evacuate at the same time, and finally apply the glue liquid to device potting or tablet molding to obtain flame-retardant, thermally conductive and insulating silicone rubber.
9. The preparation method according to claim 8, characterized in that: In steps S1 and S2, the stirring time of vacuuming while stirring is 60 minutes, and the vacuum pressure is maintained at -0.098 MPa.