Carbon fiber silica gel composite material and preparation method thereof
By adding carbon fiber composite filler and end-hydroxy silicone to carbon fiber silicone composite materials, the problem of insufficient bonding force between carbon fiber and silicone is solved, the mechanical properties and electromagnetic shielding performance of the material are improved, and its application in the field of new energy vehicles has been expanded. .
Patent Information
- Application Number
- CN202411345081.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
AI Technical Summary
The shrinkage rates of carbon fiber and silicone are inconsistent, resulting in insufficient interface binding force, affecting the mechanical properties of silicone materials, especially at low temperatures, where tensile strength and rebound resistance decrease.
By adding carbon fiber composite filler and end-hydroxy silicone to carbon fiber silicone composite materials, the cross-linking density and hardness of the material are improved, and the modification of pretreatment of carbon fiber and graphene oxide powders is enhanced to enhance the interface performance and form a three-dimensional porous structure to improve the Mechanical properties and electromagnetic shielding properties.
It significantly improves the tensile strength, rebound performance and electromagnetic shielding performance of carbon fiber silicone composite materials, and broadens its application range in the field of new energy vehicles.
Smart Images

Figure BDA0005060755010000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicone composite materials, and particularly relates to a carbon fiber silicone composite material and a preparation method thereof. Background Art
[0002] Silica gel materials can generally be divided into inorganic silica gel and organic silica gel. Inorganic silica gel is mainly used in gas drying, gas absorption, liquid dehydration, chromatography analysis and other fields. It is also often used as a catalyst carrier and dehydration and refining of organic compounds. Organic silica gel is widely used in aviation, cutting-edge technology, military technology departments, as well as construction, electronics and electrical, automobiles, machinery, chemical and light industry, medicine and medical care and other fields.
[0003] The basic structural unit of organic silicone products is composed of silicon-oxygen chain segments, and the side chains are connected to various other organic groups through silicon atoms. Therefore, organic silicone not only has the basic properties of silicone, but can also be modified according to specific needs to meet the requirements of different occasions.
[0004] Carbon fiber has the characteristics of low density, excellent mechanical properties and good thermal conductivity. In order to improve the thermal conductivity of silicone materials, micron-sized carbon fibers are generally compounded therein. However, due to the inconsistent shrinkage rates of carbon fiber and silicone, especially at low temperatures, the interface bonding strength between the silicone matrix and the carbon fiber powder is insufficient, resulting in reduced stress transfer efficiency, and the tensile strength and resilience of the product will decrease. Summary of the invention
[0005] The purpose of the present invention is to provide a carbon fiber silicone composite material and a preparation method thereof, and to improve the mechanical properties of the carbon fiber silicone composite material by adding carbon fiber composite filler and terminal hydroxyl silicone resin.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a carbon fiber silicone composite material comprises the following steps:
[0008] Add vinyl silicone oil, hydroxy silicone oil, carbon fiber composite filler, terminal hydroxy silicone resin and platinum catalyst into a homogenizer, homogenize at 1500-2000r / min for 2-3min, transfer to a mold after vacuum degassing, vulcanize at 130-135℃ for 50-60min, demold, and obtain a carbon fiber silicone composite material.
[0009] Furthermore, the mass ratio of vinyl silicone oil, hydrogenated silicone oil, hydroxy silicone oil, carbon fiber composite filler, terminal hydroxyl silicone resin and platinum catalyst is 100:40-42:5-6:2-3:1-1.5:0.05-0.1.
[0010] Further, the hydroxy-terminated silicone resin is prepared by the following steps:
[0011] Add alkaline anion exchange resin, deionized water, methylphenyldimethoxysilane, phenyltrimethoxysilane and diphenyldimethoxysilane into a reaction kettle, react at 85-90°C for 12-14h, remove the alkaline anion exchange resin as a catalyst by vacuum filtration, then let the filtrate stand for stratification, take the lower layer of reaction product and perform vacuum distillation to remove water and unreacted monomers to obtain a liquid terminal hydroxyl silicone resin.
[0012] Furthermore, the mass ratio of the basic anion exchange resin, deionized water, methylphenyldimethoxysilane, phenyltrimethoxysilane and diphenyldimethoxysilane is 40-60:90-108:182.3:198.3:244.5.
[0013] Furthermore, the carbon fiber composite filler is prepared by the following steps:
[0014] Step 1: Add carbon fiber powder and 4-6 times the mass of mixed acid into the reactor, stir for 6-8 hours at 20-25°C, then dilute with 20-30 times the volume of deionized water of the mixed acid, filter, and wash the filter cake with deionized water until the last washing liquid is neutral, so as to introduce more hydroxyl and carboxyl groups into the carbon fiber to obtain pretreated carbon fiber.
[0015] Step 2: Add graphene oxide powder, anhydrous ethanol, deionized water and silane coupling agent KH-550 into a reactor, adjust the pH value to 3 with acetic acid, stir at 200-300 r / min for 10-20 min, and then ultrasonically disperse for 20-30 min. Stir the reaction at 60-65 ° C for 5-6 h, centrifuge and filter, wash the filter cake with anhydrous ethanol 3-5 times, and vacuum dry to obtain modified graphene.
[0016] Step 3: Add the modified graphene and deionized water into the reactor and ultrasonically disperse for 20-30 minutes, then add the pretreated carbon fiber into the reactor, stir the reaction at 70-75°C and 200-300r / min for 10-12 hours, centrifuge and filter, wash the filter cake with anhydrous ethanol and deionized water for 2-3 times respectively, and vacuum dry to obtain graphene composite carbon fiber.
[0017] Step 4: Add cobalt nitrate hexahydrate, graphene composite carbon fiber and anhydrous methanol into a reactor, stir at 200-300 r / min for 20-30 min, then add 2-methylimidazole, stir and react at 35-40° C. for 22-24 h, centrifuge and filter, wash the filter cake with anhydrous methanol for 3-5 times, and vacuum dry to obtain a carbon fiber composite filler.
[0018] Furthermore, the mixed acid is prepared by mixing 95% by mass sulfuric acid and 67% by mass nitric acid in a volume ratio of 3:1.
[0019] Furthermore, the usage ratio of graphene oxide powder, anhydrous ethanol, deionized water and silane coupling agent KH-550 is 5g:45-50mL:45-50mL:0.15g.
[0020] Furthermore, the usage ratio of modified graphene, deionized water and pretreated carbon fiber is 3-3.5 g: 100-120 mL: 10 g.
[0021] Furthermore, the usage ratio of cobalt nitrate hexahydrate, graphene composite carbon fiber, anhydrous methanol and 2-methylimidazole is 12g:2-2.2g:600-800mL:22g.
[0022] Beneficial effects of the present invention:
[0023] The carbon fiber silicone composite material of the present invention uses vinyl silicone oil, hydrogenated silicone oil, hydroxyl silicone oil and the like as main raw materials, and prepares a silicone material with a three-dimensional network structure through an addition crosslinking reaction. The addition of terminal hydroxyl silicone resin helps to increase the crosslinking density of the silicone material, and the introduction of phenyl groups into the silicone product helps to increase the hardness, resilience and tensile strength of the silicone composite material.
[0024] The carbon fiber composite filler of the present invention helps to improve the thermal conductivity and electromagnetic shielding performance of the silica gel composite material. The oxygen-containing groups on the surface of the carbon fiber powder are increased after pretreatment, and the graphene oxide powder is modified by a silane coupling agent, and the amino groups grafted on the surface of the graphene oxide powder react with the carboxyl groups on the surface of the pretreated carbon fiber to load the graphene oxide on the surface of the carbon fiber to prepare the graphene composite carbon fiber. The rough surface helps to improve the interface performance between the carbon fiber and the silica gel matrix, helps to disperse the stress, and improves the mechanical properties of the silica gel composite material; the three-dimensional porous nanoparticles generated in situ by cobalt nitrate hexahydrate and 2-methylimidazole, the graphene composite carbon fiber provides more growth binding sites for it, and the graphene composite carbon fiber exhibits good electromagnetic shielding performance, which helps the application of the carbon fiber silica gel composite material in laser radar systems and battery management systems, etc., and broadens its application range in the field of new energy vehicles. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] Embodiment 1: This embodiment provides a carbon fiber silicone composite material, which is prepared by the following preparation method:
[0027] S1: Add carbon fiber powder and 4 times the mass of mixed acid into a reactor. The mixed acid is prepared by mixing 95% sulfuric acid and 67% nitric acid in a volume ratio of 3:1. Stir at 20°C for 6 hours, then dilute with 20 times the volume of deionized water, filter, and wash the filter cake with deionized water until the last washing liquid is neutral, so as to introduce more hydroxyl and carboxyl groups into the carbon fiber to obtain pretreated carbon fiber.
[0028] S2: 5 kg of graphene oxide powder, 45 L of anhydrous ethanol, 45 L of deionized water and 0.15 kg of silane coupling agent KH-550 were added to a reactor, the pH value was adjusted to 3 with acetic acid, stirred at 200 r / min for 10 min and then ultrasonically dispersed for 20 min, stirred and reacted at 60 ° C for 5 h, centrifuged and filtered, the filter cake was washed 3 times with anhydrous ethanol, and vacuum dried to obtain modified graphene.
[0029] S3: 3 kg of modified graphene and 100 L of deionized water were added to the reactor and ultrasonically dispersed for 20 min. Then, 10 kg of pretreated carbon fiber was added to the reactor, stirred and reacted at 70 ° C and 200 r / min for 10 h, centrifuged and filtered, and the filter cake was washed twice with anhydrous ethanol and deionized water respectively, and vacuum dried to obtain graphene composite carbon fiber.
[0030] S4: 12 kg of cobalt nitrate hexahydrate, 2 kg of graphene composite carbon fiber and 600 L of anhydrous methanol were added into a reactor, stirred at 200 r / min for 20 min, and then 22 kg of 2-methylimidazole was added, stirred and reacted at 35 ° C for 22 h, centrifuged and filtered, the filter cake was washed 3 times with anhydrous methanol, and vacuum dried to obtain a carbon fiber composite filler.
[0031] S5: Add 4kg of alkaline anion exchange resin, 9kg of deionized water, 18.23kg of methylphenyldimethoxysilane, 19.83kg of phenyltrimethoxysilane and 24.45kg of diphenyldimethoxysilane into the reactor, react at 85°C for 12h, filter under reduced pressure to remove the alkaline anion exchange resin as a catalyst, then let the filtrate stand to separate layers, take the lower layer of reaction product and distill under reduced pressure to remove water and unreacted monomers to obtain a liquid terminal hydroxyl silicone resin.
[0032] S6: Add 10kg vinyl silicone oil, 4kg hydrogenated silicone oil, 0.5kg hydroxyl silicone oil, 0.2kg carbon fiber composite filler, 0.1kg terminal hydroxyl silicone resin and 5g platinum catalyst into a homogenizer, homogenize at 1500r / min for 2min, transfer to a mold after vacuum degassing, vulcanize at 130°C for 50min, and demold to obtain a carbon fiber silicone composite material.
[0033] Embodiment 2: This embodiment provides a carbon fiber silicone composite material, which is prepared by the following preparation method:
[0034] S1: Add carbon fiber powder and 5 times the mass of mixed acid into a reactor. The mixed acid is prepared by mixing 95% sulfuric acid and 67% nitric acid in a volume ratio of 3:1. Stir at 22°C for 7 hours, then dilute with 25 times the volume of deionized water, filter, and wash the filter cake with deionized water until the last washing liquid is neutral, so as to introduce more hydroxyl and carboxyl groups into the carbon fiber to obtain pretreated carbon fiber.
[0035] S2: 5 kg of graphene oxide powder, 48 L of anhydrous ethanol, 48 L of deionized water and 0.15 kg of silane coupling agent KH-550 were added to a reactor, the pH value was adjusted to 3 with acetic acid, stirred at 250 r / min for 15 min and then ultrasonically dispersed for 25 min, stirred and reacted at 62 ° C for 5.5 h, centrifuged and filtered, the filter cake was washed 4 times with anhydrous ethanol, and vacuum dried to obtain modified graphene.
[0036] S3: 3.25 kg of modified graphene and 110 L of deionized water were added to the reactor and ultrasonically dispersed for 25 min. Then, 10 kg of pretreated carbon fiber was added to the reactor, stirred and reacted at 72 ° C and 250 r / min for 11 h, centrifuged and filtered, and the filter cake was washed twice with anhydrous ethanol and deionized water respectively, and vacuum dried to obtain graphene composite carbon fiber.
[0037] S4: 12 kg of cobalt nitrate hexahydrate, 2.1 kg of graphene composite carbon fiber and 700 L of anhydrous methanol were added into a reactor, stirred at 250 r / min for 25 min, and then 22 kg of 2-methylimidazole was added, stirred and reacted at 38 ° C for 23 h, centrifuged and filtered, the filter cake was washed 4 times with anhydrous methanol, and vacuum dried to obtain a carbon fiber composite filler.
[0038] S5: Add 5kg of alkaline anion exchange resin, 9.9kg of deionized water, 18.23kg of methylphenyldimethoxysilane, 19.83kg of phenyltrimethoxysilane and 24.45kg of diphenyldimethoxysilane into the reactor, react at 88°C for 13h, filter under reduced pressure to remove the alkaline anion exchange resin as a catalyst, then let the filtrate stand to separate layers, take the lower layer of reaction product and distill under reduced pressure to remove water and unreacted monomers to obtain a liquid terminal hydroxyl silicone resin.
[0039] S6: Add 10kg vinyl silicone oil, 4.1kg hydrogenated silicone oil, 0.55kg hydroxyl silicone oil, 0.25kg carbon fiber composite filler, 0.14kg terminal hydroxyl silicone resin and 8g platinum catalyst into a homogenizer, homogenize at 1800r / min for 2.5min, transfer to a mold after vacuum degassing, vulcanize at 132°C for 55min, and demold to obtain a carbon fiber silicone composite material.
[0040] Embodiment 3: This embodiment provides a carbon fiber silicone composite material, which is prepared by the following preparation method:
[0041] S1: Add carbon fiber powder and 6 times the mass of mixed acid into a reactor. The mixed acid is prepared by mixing 95% sulfuric acid and 67% nitric acid in a volume ratio of 3:1. Stir at 25°C for 8 hours, then dilute with 30 times the volume of deionized water, filter, and wash the filter cake with deionized water until the last washing liquid is neutral, so as to introduce more hydroxyl and carboxyl groups into the carbon fiber to obtain pretreated carbon fiber.
[0042] S2: 5 kg of graphene oxide powder, 50 L of anhydrous ethanol, 50 L of deionized water and 0.15 kg of silane coupling agent KH-550 were added to a reactor, the pH value was adjusted to 3 with acetic acid, stirred at 300 r / min for 20 min and then ultrasonically dispersed for 30 min, stirred and reacted at 65 ° C for 6 h, centrifuged and filtered, the filter cake was washed 5 times with anhydrous ethanol, and vacuum dried to obtain modified graphene.
[0043] S3: 3.5 kg of modified graphene and 120 L of deionized water were added to the reactor and ultrasonically dispersed for 30 min. Then, 10 kg of pretreated carbon fiber was added to the reactor, stirred and reacted at 75 ° C and 300 r / min for 12 h, centrifuged and filtered, and the filter cake was washed 3 times with anhydrous ethanol and deionized water respectively, and vacuum dried to obtain graphene composite carbon fiber.
[0044] S4: 12 kg of cobalt nitrate hexahydrate, 2.2 kg of graphene composite carbon fiber and 800 L of anhydrous methanol were added into a reactor, stirred at 300 r / min for 30 min, and then 22 kg of 2-methylimidazole was added, stirred and reacted at 40° C. for 24 h, centrifuged and filtered, the filter cake was washed 5 times with anhydrous methanol, and vacuum dried to obtain a carbon fiber composite filler.
[0045] S5: Add 6kg of alkaline anion exchange resin, 10.8kg of deionized water, 18.23kg of methylphenyldimethoxysilane, 19.83kg of phenyltrimethoxysilane and 24.45kg of diphenyldimethoxysilane into the reactor, react at 90°C for 14h, filter under reduced pressure to remove the alkaline anion exchange resin used as a catalyst, then let the filtrate stand to separate into layers, take the lower layer of reaction product and distill under reduced pressure to remove water and unreacted monomers to obtain a liquid terminal hydroxyl silicone resin.
[0046] S6: Add 10kg vinyl silicone oil, 4.2kg hydrogenated silicone oil, 0.6kg hydroxyl silicone oil, 0.3kg carbon fiber composite filler, 0.18kg terminal hydroxyl silicone resin and 10g platinum catalyst into a homogenizer, homogenize at 2000r / min for 3min, transfer to a mold after vacuum degassing, vulcanize at 135°C for 60min, and demold to obtain a carbon fiber silicone composite material.
[0047] Comparative Example 1: Based on Example 3, no hydroxyl-terminated silicone resin was added, and the other steps remained unchanged to prepare a carbon fiber silicone composite material.
[0048] Comparative Example 2: Based on Example 3, the carbon fiber composite filler is directly replaced by carbon fiber powder in step S6, and the other steps remain unchanged to prepare a carbon fiber silicone composite material.
[0049] Comparative Example 3: Based on Example 3, step S6 uses the graphene composite carbon fiber in step S4 to replace the carbon fiber composite filler, and the other steps remain unchanged to prepare a carbon fiber silicone composite material.
[0050] Comparative Example 4: Based on Example 3, no carbon fiber composite filler was added, and the other steps remained unchanged to prepare a silica gel composite material.
[0051] Performance tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3. Corresponding samples were prepared according to the reference standards. The tensile strength of different samples was tested with reference to GB / T 528-2009; the thermal conductivity of different samples was tested with reference to ASTM D5470-2017; the electromagnetic shielding effectiveness of different samples was tested with reference to GJB 6190-2008, and the electromagnetic wave frequency range was 30MHz-18GHz; the compression permanent deformation rate of different samples was tested with reference to ASTM D3951; and the hardness (Shao A) of different samples was tested with reference to GB / T 531.1-2008. The results are shown in Table 1:
[0052] Table 1
[0053]
[0054] It can be seen from Table 1 that the samples in Examples 1 to 3 have higher tensile strength and better electromagnetic shielding performance. Combined with Comparative Example 1, it is shown that the hydroxyl-terminated silicone resin helps to increase the mechanical strength of the silicone composite material and improve the resilience of the silicone material; combined with Comparative Examples 2 to 4, it is shown that the carbon fiber composite filler helps to improve the electromagnetic shielding performance and thermal conductivity of the silicone composite material.
[0055] It should be noted that, in this article, terms such as "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a carbon fiber silicone composite material, characterized in that: The steps include: Step 1: Add modified graphene and deionized water into a reactor and ultrasonically disperse for 20-30 minutes, add pretreated carbon fiber, stir and react at 70-75°C and 200-300r / min for 10-12 hours, centrifuge and filter, wash the filter cake, and vacuum dry to obtain graphene composite carbon fiber; Step 2: Add cobalt nitrate hexahydrate, graphene composite carbon fiber and anhydrous methanol into a reaction kettle, stir at 200-300 r / min for 20-30 min, add 2-methylimidazole, stir at 35-40° C. for 22-24 h, centrifuge and filter, wash the filter cake, and vacuum dry to obtain a carbon fiber composite filler; Step 3: Add vinyl silicone oil, hydroxy silicone oil, carbon fiber composite filler, terminal hydroxy silicone resin and platinum catalyst into a homogenizer, homogenize at 1500-2000r / min for 2-3min, transfer to a mold after vacuum degassing, vulcanize at 130-135℃ for 50-60min, demold, and obtain a carbon fiber silicone composite material; The mass ratio of the vinyl silicone oil, hydrogen-containing silicone oil, hydroxy silicone oil, carbon fiber composite filler, terminal hydroxyl silicone resin and platinum catalyst is 100:40-42:5-6:2-3:1-1.5:0.05-0.
1.
2. The method for preparing a carbon fiber silicone composite material according to claim 1, characterized in that: The usage ratio of the modified graphene, deionized water and pretreated carbon fiber is 3-3.5 g: 100-120 mL: 10 g.
3. The method for preparing a carbon fiber silicone composite material according to claim 1, characterized in that: The usage ratio of the cobalt nitrate hexahydrate, the graphene composite carbon fiber, the anhydrous methanol and the 2-methylimidazole is 12g:2-2.2g:600-800mL:22g.
4. The method for preparing a carbon fiber silicone composite material according to claim 1, characterized in that: The hydroxy-terminated silicone resin is prepared by the following steps: Add alkaline anion exchange resin, deionized water, methylphenyldimethoxysilane, phenyltrimethoxysilane and diphenyldimethoxysilane into the reaction kettle, react at 85-90°C for 12-14 hours, filter under reduced pressure, let the filtrate stand for stratification, take the lower layer of reaction product and distill under reduced pressure to remove water and unreacted monomers to obtain a liquid terminal hydroxyl silicone resin.
5. The method for preparing a carbon fiber silicone composite material according to claim 4, characterized in that: The mass ratio of the alkaline anion exchange resin, deionized water, methylphenyldimethoxysilane, phenyltrimethoxysilane and diphenyldimethoxysilane is 40-60:90-108:182.3:198.3:244.
5.
6. The method for preparing a carbon fiber silicone composite material according to claim 1, characterized in that: The pretreated carbon fiber is prepared by the following steps: Add carbon fiber powder and 4-6 times the mass of mixed acid into a reactor, stir at 20-25°C for 6-8h, then dilute with 20-30 times the volume of deionized water of the mixed acid, filter, and wash the filter cake with deionized water until the last washing liquid is neutral to obtain pretreated carbon fiber.
7. The method for preparing a carbon fiber silicone composite material according to claim 6, characterized in that: The mixed acid is prepared by mixing 95% by mass sulfuric acid and 67% by mass nitric acid in a volume ratio of 3:
1.
8. The method for preparing a carbon fiber silicone composite material according to claim 1, characterized in that: The modified graphene is prepared by the following steps: Add graphene oxide powder, anhydrous ethanol, deionized water and silane coupling agent KH-550 into a reactor, adjust the pH value to 3 with acetic acid, stir at 200-300 r / min for 10-20 min, then ultrasonically disperse for 20-30 min, stir and react at 60-65° C. for 5-6 h, centrifuge and filter, wash the filter cake, and vacuum dry to obtain modified graphene.
9. The method for preparing a carbon fiber-silicone composite material according to claim 8, characterized in that: The usage ratio of the graphene oxide powder, anhydrous ethanol, deionized water and silane coupling agent KH-550 is 5g:45-50mL:45-50mL:0.15g.
10. A carbon fiber silicone composite material, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 9.