Preparation method of nano-composite coating on surface of crystallizer copper plate

By preparing nanocomposite coatings on the surface of the copper plate of the crystallizer, using materials such as tungsten carbide, tungsten, titanium carbide, cobalt, iron carbonyl carbonyl carbonyl, nickel carbonyl oxide, zirconium oxide and titanium carbonitride, the existing coatings are solved in high-temperature casting Cu Ion diffusion, wear and splashing problems improve hardness and wear resistance and extend service life.

CN119081455AActive Publication Date: 2024-12-06武汉钢铁有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411325628.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-06
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

The existing surface coating of copper plates of crystallizers has problems in Cu ion diffusion and infiltration, wear and splashing of the lower part of the crystallizer in high-temperature casting, and the existing coating has defects in wear resistance, bonding and hardness, which affects the service life.

Method used

The preparation method of nanocomposite coatings includes the use of tungsten carbide powder, tungsten powder and titanium carbide powder as basic hardness aggregates, cobalt powder, iron carbonyl carbonyl carbonyl carbonyl carbonyl and nickel carbonyl powder as high-active binding agents, nanozirconia powder and nanocarbon As a nanoadditive, titanium nitride powder forms a nanocomposite coating through wet ball milling, stirring, ultrasonic dispersion, vacuum hot press sintering and spraying techniques to improve the hardness, wear resistance and bonding of the coating.

Benefits of technology

The coating has achieved high hardness (HV 500~800), high wear resistance and excellent combination performance, extending the service life of the crystallizer copper plate, and the single over-steel volume has increased to 80,000 ton/set, and its service life is It reaches 2800~3500 furnaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081455A_ABST
    Figure CN119081455A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of composite coatings, and discloses a preparation method of a nano composite coating on the surface of a crystallizer copper plate. The preparation method comprises the following steps: firstly, premixing the basic hardness aggregate, the high-activity binding agent and the nano additive according to respective raw material composition; carrying out wet ball milling on the basic hardness aggregate, sequentially adding the high-activity binding agent and the nano additive, and stirring to obtain mixed slurry; then, the mixed slurry is dried, sieved and sintered, a sintered product is crushed, and nano-composite coating powder is obtained; and finally, spraying the nano-composite coating powder on the surface of a crystallizer copper plate base material to form the nano-composite coating. A hard phase generated by the basic hardness aggregate and a binding phase generated by the nano additive enable the coating to have higher hardness and wear resistance, and the high-activity binding agent enables the hard phase and the binding phase as well as the hard phase and the binding phase and a crystallizer copper plate matrix to have better binding property, so that the coating is excellent in comprehensive performance and stable in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite coatings, and in particular relates to a method for preparing a nano composite coating on the surface of a crystallizer copper plate. Background Art

[0002] The crystallizer is the core component of continuous casting. The copper plate of the crystallizer is an important heat-conducting component from liquid steel to solidified solid billet shell. Its quality directly affects the surface quality of the billet, the casting speed of the continuous casting machine and other indicators. The molten steel flows through the copper plate of the crystallizer, crystallizes into billets under the action of external cooling water, and is pulled out of the crystallizer by the dummy rod. Frequent billet drawing causes serious wear of the copper plate of the crystallizer, and frequent replacement not only reduces production efficiency, but also consumes a large number of crystallizers. In order to improve the service life of the copper plate of the crystallizer, relevant units and experts at home and abroad have made a lot of efforts in the material of the copper plate, which has greatly improved the high-temperature strength and hardness. However, it still cannot solve the problems of diffusion and infiltration of Cu ions during high-temperature casting, wear of the lower part of the crystallizer, and splashing when pouring. The effective way to solve these problems is the coating on the surface of the copper plate.

[0003] In the early stage of coating research, Cr coating was proposed from the perspective of wear resistance and splash resistance, but Cr coating is easy to peel off when it is thick. In order to solve the coating thickness, Ni-Cr composite coating was proposed. Since the thermal expansion coefficient of Ni is close to that of Cu, the peeling problem is improved and the thickness can be increased. However, it was found in actual use that due to the increase in casting speed and the close contact of the billet shell under the static pressure of molten iron, the mechanical friction load increased, resulting in the problem of wear on the lower part of the crystallizer not being satisfactorily solved. In order to further improve the wear resistance of the coating and increase the service life of the crystallizer copper plate, Ni-Fe coating, Ni-Co coating and Co-Ni coating were developed thereafter. However, the hardness of Ni-Fe coating is only between HV 250 and 550. When the hardness is high, the coating stress of Ni-Co coating and Co-Ni coating is large, and the thermal alternation resistance is poor, which affects its long-term stability and reliability. In general, in order to achieve a long life of the crystallizer, it has become a trend to prepare a wear-resistant coating on the surface of the crystallizer, but the existing coatings still have defects in terms of bonding, wear resistance, hardness, and stable performance. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing a nano-composite coating on the surface of a crystallizer copper plate in view of the deficiencies in the prior art. The raw materials of the nano-composite coating include basic hardness aggregate, nano-additives and high-activity binders. After being sprayed on the surface of the crystallizer copper plate, the hard phase generated by the basic hardness aggregate and the binding phase generated by the nano-additives make the coating have higher hardness and wear resistance. The high-activity binder makes the hard phase and the binding phase and the two have better bonding with the crystallizer copper plate matrix, so that the coating has excellent comprehensive performance and stable performance.

[0005] In order to solve the technical problem proposed by the present invention, the present invention provides a method for preparing a nano-composite coating on the surface of a crystallizer copper plate, comprising the following steps:

[0006] 1) Premix tungsten carbide powder, tungsten powder and titanium carbide powder to obtain basic hardness aggregate;

[0007] 2) premixing cobalt powder, carbonyl iron powder and carbonyl nickel powder to obtain a highly active binder;

[0008] 3) Premixing nano zirconium oxide powder and nano titanium carbonitride powder to obtain a nano additive;

[0009] 4) wet-milling the basic hardness aggregate, then adding a high-activity binder for primary stirring, then adding a nano-additive for secondary stirring, and finally performing ultrasonic dispersion to obtain a mixed slurry;

[0010] 5) drying the mixed slurry and sieving it, and then sintering it by vacuum hot pressing or vacuum hot isostatic pressing, crushing the sintered product to obtain a nanocomposite coating powder;

[0011] 6) The surface of the copper plate substrate of the crystallizer is treated to make the rust removal and roughness meet the spraying requirements, and the nano-composite coating powder is sprayed onto the surface of the copper plate substrate of the crystallizer by supersonic flame spraying or plasma spraying to form a nano-composite coating.

[0012] In the above solution, the purity of the tungsten carbide powder is greater than 99% and the particle size is less than 3 μm.

[0013] In the above solution, the purity of the tungsten powder is greater than 99% and the particle size is less than 1 μm.

[0014] In the above solution, the purity of the titanium carbide powder is greater than 99% and the particle size is less than 1 μm.

[0015] In the above scheme, the mass ratio of the tungsten carbide powder, tungsten powder and titanium carbide powder is (4-6):(1-2):1.

[0016] Preferably, the mass ratio of the tungsten carbide powder, tungsten powder and titanium carbide powder is (4-5):(1-2):1.

[0017] In the above solution, the purity of the cobalt powder is greater than 99% and the particle size is less than 1 μm.

[0018] In the above scheme, the purity of the carbonyl iron powder is greater than 99% and the particle size is less than 2 μm.

[0019] In the above scheme, the purity of the carbonyl nickel powder is greater than 99% and the particle size is less than 2 μm.

[0020] In the above scheme, the mass ratio of the cobalt powder, the carbonyl iron powder and the carbonyl nickel powder is 1:(1-3):(1-3).

[0021] Preferably, the mass ratio of the cobalt powder, the carbonyl iron powder and the carbonyl nickel powder is 1:(1-2.5):(1-2.5).

[0022] In the above scheme, the purity of the nano zirconium oxide powder is greater than 99%, and the particle size is 20-60 nm.

[0023] In the above scheme, the purity of the nano titanium carbonitride powder is greater than 99%, and the particle size is 50-200nm.

[0024] In the above scheme, the mass ratio of the nano zirconium oxide powder to the nano titanium carbonitride powder is 1:(2-4).

[0025] Preferably, the mass ratio of the nano zirconium oxide powder to the nano titanium carbonitride powder is 1:(2-3).

[0026] In the above scheme, the wet ball milling adopts a planetary ball mill, anhydrous ethanol is used as the ball milling medium, and is equipped with a stainless steel ball milling jar and a high-hardness metal ball mill. The ball milling speed is 50-100r / min and the ball milling time is 30-60h.

[0027] In the above scheme, the stirring is carried out using a V-type mixer; the stirring rate of the first stirring is 50-60 r / min, and the stirring time is 0.5-1 h; the stirring rate of the second stirring is 80-10 r / min, and the stirring time is 4.5-9 h.

[0028] In the above scheme, the ultrasonic dispersion treatment time is 10 to 30 minutes.

[0029] In the above scheme, the mass of the high-activity binder is 10-20% of the mass of the basic hardness aggregate.

[0030] Preferably, the mass of the high-activity binder is 10-18% of the mass of the basic hardness aggregate.

[0031] In the above scheme, the mass of the nano additive is 1-5% of the mass of the basic hardness aggregate.

[0032] Preferably, the mass of the nano-additive is 1-3.5% of the mass of the basic hardness aggregate.

[0033] In the above scheme, the mixed slurry is dried and sieved with 250-320 meshes to take the sieve residue.

[0034] In the above scheme, the vacuum degree of the vacuum hot pressing sintering or vacuum hot isostatic pressing sintering is 3.5×10 -3 ~4.5×10 -3Pa, the sintering temperature is 1400-1500℃, the pressure is 20-40MPa, and the holding time is 1-3h.

[0035] Preferably, the vacuum degree of the vacuum hot isostatic pressing sintering is 3.6×10 -3 ~4.3×10 -3 Pa, the sintering temperature is 1410-1490℃, the pressure is 20-35MPa, and the holding time is 1-2.5h.

[0036] In the above solution, the particle size of the nanocomposite coating powder is less than 10 μm.

[0037] In the above scheme, the crystallizer copper plate substrate is Ag-Cu alloy or Cu-Cr-Zr alloy.

[0038] Furthermore, when the crystallizer copper plate substrate is an Ag-Cu alloy, its chemical composition by mass percentage includes: Cu>99.5%, Ag 0.05% to 0.1%, and the rest are unavoidable impurities.

[0039] Furthermore, when the copper plate substrate of the crystallizer is a Cu-Cr-Zr alloy, its chemical composition by mass percentage includes: Cu>98%, Cr 0.5-1.5%, Zr 0.01-0.3%, and the rest are unavoidable impurities.

[0040] In the above scheme, the rust removal grade of the crystallizer copper plate substrate is Sa3, St2 or St3, and the roughness should reach 2.5-5 μmRa.

[0041] In the above solution, the thickness of the nanocomposite coating is 1.5 to 3 mm.

[0042] In the above scheme, the density of the nano-composite coating is greater than 99.7%, the hardness HV is 500-800, the bonding strength between the nano-composite coating and the crystallizer copper plate substrate is 200-400MPa, the crystallizer copper plate with the nano-composite coating has a single steel passing capacity of 80,000-150,000 tons / set, and a service life of 2,800-3,500 furnaces.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] The present invention uses basic hardness aggregates composed of tungsten carbide, tungsten and titanium carbide as main raw materials, and the generated hard phase can give the coating a high basic hardness; then nano additives composed of nano zirconium oxide and nano titanium carbonitride, and high-activity binders composed of cobalt, carbonyl iron and carbonyl nickel are added between the aggregates to generate Ni-W / ZrO2, Ni-TiC, WC-Ni, Ni-W-WC, Fe-Ni / ZrO2, Fe-Ni-Ti(C, N)-WC and other intermediate phases between the matrix gaps, thereby improving the compactness of the coating composite; the amorphous binding phase generated by the nano additive wraps the hard phase, To further improve the hardness and wear resistance, nano ZrO2 and nano TiCN can also form a gradient interlaced arrangement with the matrix at the grain boundary of the matrix, further enhancing the hardness and wear resistance at the grain boundary; Ni, Fe and Co in the high-activity binder can enhance the bonding strength between the hard phase and the bonding phase and between the coating and the crystallizer copper plate matrix, and hydroxyl iron powder and hydroxyl nickel powder can also improve the sintering tightness of the hard phase and the bonding phase between the coating, and also help to improve the bonding performance between the coating and the copper plate during the spraying process; the combined effect of the above raw materials makes the coating have excellent comprehensive performance and stable performance, thereby giving the crystallizer copper plate a long service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the cross-sectional microstructure of the nanocomposite coating prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0046] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.

[0047] In the following examples, the density of the surface coating was tested using the "GB / T 25995-2010 Fine Ceramics Density and Apparent Porosity Test Method"; the hardness of the surface coating was tested using the "GB / T 16534-2009 Fine Ceramics Room Temperature Hardness Test Method"; and the bonding strength between the surface coating and the crystallizer copper plate substrate was tested using the "GB / T 6569-2006 Fine Ceramics Bending Strength Test Method".

[0048] Example 1

[0049] The raw materials involved in this embodiment are as follows:

[0050] The purity of tungsten carbide powder is 99.7%, and the particle size is 2μm; the purity of tungsten powder is 99.8%, and the particle size is 0.5μm; the purity of titanium carbide powder is 99.8%, and the particle size is 0.5μm; the purity of cobalt powder is 99.5%, and the particle size is 0.8μm; the purity of carbonyl iron powder is 99.5%, and the particle size is 0.8μm; the purity of carbonyl nickel powder is 99.5%, and the particle size is 1μm; the purity of nano zirconium oxide powder is 99.5%, and the particle size is 50nm; the purity of nano titanium carbonitride powder is 99.5%, and the particle size is 80nm.

[0051] The materials involved in this embodiment are as follows:

[0052] The crystallizer copper plate substrate is Ag-Cu alloy, and its chemical composition includes, by mass percentage: Cu 99.8%, Ag 0.08%, and the rest are inevitable impurities.

[0053] The method for preparing the nano-composite coating on the surface of the crystallizer copper plate in this embodiment comprises the following steps:

[0054] 1) Mix tungsten carbide powder, tungsten powder and titanium carbide powder in a mass ratio of 4:1:1 to obtain a basic hardness aggregate;

[0055] 2) mixing cobalt powder, carbonyl iron powder and carbonyl nickel powder in a mass ratio of 1:1:1 to obtain a highly active binder;

[0056] 3) mixing nano zirconium oxide powder and nano titanium carbonitride powder in a mass ratio of 1:2 to obtain a nano additive;

[0057] 4) using a planetary ball mill, anhydrous ethanol as the ball milling medium, equipped with a stainless steel ball mill and a high-hardness metal ball mill, the basic hardness aggregate is wet-milled at a ball milling speed of 60 r / min for 48 h; the milled material is transferred to a V-type mixer, a high-activity binder of 12% of the mass of the basic hardness aggregate is added and stirred at 60 r / min for 0.75 h, and then a nano-additive of 1.5% of the mass of the basic hardness aggregate is added and stirred at 85 r / min for 8 h; the stirred material is introduced into a glass container, and an ultrasonic device is used to disperse it for 15 min to obtain a mixed slurry;

[0058] 5) After the mixed slurry is dried, it is passed through a 250-mesh sieve, and the sieve material is taken out, and then vacuum hot pressing sintering is performed, and the vacuum degree is 3.9×10 -3 Pa, sintering temperature is 1450℃, hot pressing pressure is 25MPa, holding time is 2h, the sintered product is crushed to obtain nanocomposite coating powder with a particle size of 8μm;

[0059] 6) The surface of the copper plate substrate of the crystallizer is treated, the rust removal grade is Sa3, and the roughness reaches 2.5 μmRa. The nano-composite coating powder is sprayed onto the surface of the copper plate substrate of the crystallizer by supersonic flame spraying to form a nano-composite coating with a thickness of 2 mm.

[0060] Figure 1 This is the cross-sectional microstructure of the nanocomposite coating prepared in this embodiment. It can be seen from the figure that the coating has good uniformity in phase composition, wherein the hard phase (black area) formed by the basic hardness aggregate is encapsulated by the amorphous bonding phase (gray area) generated by the nano-additive, thereby improving the hardness and wear resistance of the coating.

[0061] After testing, the density of the nano-composite coating prepared in this embodiment is 99.8%, the hardness HV reaches 550, the bonding strength between the nano-composite coating and the crystallizer copper plate substrate is 295 MPa, and the actual single-time steel passing capacity of the crystallizer copper plate with the nano-composite coating is 95,000 tons / set, and the service life is 3,100 furnaces.

[0062] Example 2

[0063] The raw materials involved in this embodiment are as follows:

[0064] The purity of tungsten carbide powder is 99.8%, and the particle size is 1μm; the purity of tungsten powder is 99.7%, and the particle size is 0.8μm; the purity of titanium carbide powder is 99.7%, and the particle size is 0.8μm; the purity of cobalt powder is 99.6%, and the particle size is 0.5μm; the purity of carbonyl iron powder is 99.6%, and the particle size is 1μm; the purity of carbonyl nickel powder is 99.6%, and the particle size is 1μm; the purity of nano zirconium oxide powder is 99.6%, and the particle size is 50nm; the purity of nano titanium carbonitride powder is 99.6%, and the particle size is 100nm.

[0065] The materials involved in this embodiment are as follows:

[0066] The crystallizer copper plate substrate is Ag-Cu alloy, and its chemical composition includes, by mass percentage: Cu 99.7%, Ag 0.06%, and the rest are inevitable impurities.

[0067] The method for preparing the nano-composite coating on the surface of the crystallizer copper plate in this embodiment comprises the following steps:

[0068] 1) Mix tungsten carbide powder, tungsten powder and titanium carbide powder in a mass ratio of 5:1.5:1 to obtain a basic hardness aggregate;

[0069] 2) mixing cobalt powder, carbonyl iron powder and carbonyl nickel powder in a mass ratio of 1:1:2 to obtain a highly active binder;

[0070] 3) mixing nano zirconium oxide powder and nano titanium carbonitride powder in a mass ratio of 1:2.5 to obtain a nano additive;

[0071] 4) using a planetary ball mill, anhydrous ethanol as the ball milling medium, equipped with a stainless steel ball mill and a high-hardness metal ball mill, the basic hardness aggregate is wet-milled at a ball milling speed of 80 r / min for 50 h; the milled material is transferred to a V-type mixer, a high-activity binder of 18% of the mass of the basic hardness aggregate is added and stirred at 50 r / min for 1 h, and then a nano-additive of 3% of the mass of the basic hardness aggregate is added and stirred at 90 r / min for 8.5 h; the stirred material is introduced into a glass container, and an ultrasonic device is used to disperse it for 20 min to obtain a mixed slurry;

[0072] 5) After the mixed slurry is dried, it is passed through a 280-mesh sieve, and the sieve material is taken out, and then vacuum hot pressing sintering is performed, and the vacuum degree is 4×10 -3 Pa, sintering temperature is 1440℃, hot pressing pressure is 35MPa, holding time is 1.5h, the sintered product is crushed to obtain nanocomposite coating powder with a particle size of 5μm;

[0073] 6) The surface of the copper plate substrate of the crystallizer is treated, the rust removal grade is St2, and the roughness reaches 3 μmRa. The nano-composite coating powder is sprayed onto the surface of the copper plate substrate of the crystallizer by supersonic flame spraying to form a nano-composite coating with a thickness of 1.6 mm.

[0074] After testing, the density of the nano-composite coating prepared in this embodiment is 99.8%, the hardness HV reaches 620, the bonding strength between the nano-composite coating and the crystallizer copper plate substrate is 350MPa, and the actual single-time steel passing capacity of the crystallizer copper plate with the nano-composite coating is 115,000 tons / set, and the service life is 3,200 furnaces.

[0075] Example 3

[0076] The raw materials involved in this embodiment are as follows:

[0077] The purity of tungsten carbide powder is 99.5%, and the particle size is 2μm; the purity of tungsten powder is 99.5%, and the particle size is 0.3μm; the purity of titanium carbide powder is 99.5%, and the particle size is 0.3μm; the purity of cobalt powder is 99.5%, and the particle size is 0.5μm; the purity of carbonyl iron powder is 99.5%, and the particle size is 1μm; the purity of carbonyl nickel powder is 99.5%, and the particle size is 1μm; the purity of nano zirconium oxide powder is 99.5%, and the particle size is 30nm; the purity of nano titanium carbonitride powder is 99.5%, and the particle size is 150nm.

[0078] The materials involved in this embodiment are as follows:

[0079] The copper plate substrate of the crystallizer is a Cu-Cr-Zr alloy, and its chemical composition includes, by mass percentage, Cu 98.8%, Cr 1%, Zr 0.02%, and the rest are inevitable impurities.

[0080] The method for preparing the nano-composite coating on the surface of the crystallizer copper plate in this embodiment comprises the following steps:

[0081] 1) Mix tungsten carbide powder, tungsten powder and titanium carbide powder in a mass ratio of 5:1:1 to obtain a basic hardness aggregate;

[0082] 2) mixing cobalt powder, carbonyl iron powder and carbonyl nickel powder in a mass ratio of 1:2:1 to obtain a highly active binder;

[0083] 3) mixing nano zirconium oxide powder and nano titanium carbonitride powder in a mass ratio of 1:3 to obtain a nano additive;

[0084] 4) using a planetary ball mill, anhydrous ethanol as the ball milling medium, equipped with a stainless steel ball mill and a high-hardness metal ball mill, the basic hardness aggregate is wet-milled at a ball milling speed of 100 r / min for 30 h; the milled material is transferred to a V-type mixer, a high-activity binder of 18% of the mass of the basic hardness aggregate is added and stirred at 55 r / min for 1 h, and then a nano-additive of 1.5% of the mass of the basic hardness aggregate is added and stirred at 100 r / min for 7.5 h; the stirred material is introduced into a glass container, and an ultrasonic device is used to disperse it for 25 min to obtain a mixed slurry;

[0085] 5) After the mixed slurry is dried, it is passed through a 320-mesh sieve, and the sieve material is taken out, and then vacuum hot isostatic pressing is performed, and the vacuum degree is 4.3×10 -3 Pa, sintering temperature is 1460℃, sintering pressure is 35MPa, holding time is 2h, the sintered product is crushed to obtain nanocomposite coating powder with a particle size of 5μm;

[0086] 6) The surface of the copper plate substrate of the crystallizer is treated, the rust removal grade is St2, and the roughness reaches 3.5 μmRa. The nano-composite coating powder is sprayed onto the surface of the copper plate substrate of the crystallizer by supersonic flame spraying to form a nano-composite coating with a thickness of 2.5 mm.

[0087] After testing, the density of the nano-composite coating prepared in this embodiment is 99.9%, the hardness HV reaches 710, the bonding strength between the nano-composite coating and the crystallizer copper plate substrate is 380 MPa, and the actual single-time steel passing capacity of the crystallizer copper plate with the nano-composite coating is 125,000 tons / set, and the service life is 3,300 furnaces.

[0088] Example 4

[0089] The raw materials involved in this embodiment are as follows:

[0090] The purity of tungsten carbide powder is 99.8%, and the particle size is 1μm; the purity of tungsten powder is 99.8%, and the particle size is 0.5μm; the purity of titanium carbide powder is 99.8%, and the particle size is 0.5μm; the purity of cobalt powder is 99.6%, and the particle size is 0.2μm; the purity of carbonyl iron powder is 99.6%, and the particle size is 0.2μm; the purity of carbonyl nickel powder is 99.6%, and the particle size is 1μm; the purity of nano zirconium oxide powder is 99.6%, and the particle size is 30nm; the purity of nano titanium carbonitride powder is 99.6%, and the particle size is 60nm.

[0091] The materials involved in this embodiment are as follows:

[0092] The copper plate substrate of the crystallizer is a Cu-Cr-Zr alloy, and its chemical composition includes, by mass percentage, Cu 98.8%, Cr 0.6%, Zr 0.015%, and the rest are inevitable impurities.

[0093] The method for preparing the nano-composite coating on the surface of the crystallizer copper plate in this embodiment comprises the following steps:

[0094] 1) Mix tungsten carbide powder, tungsten powder and titanium carbide powder in a mass ratio of 5:1:1 to obtain a basic hardness aggregate;

[0095] 2) mixing cobalt powder, carbonyl iron powder and carbonyl nickel powder in a mass ratio of 1:2.5:1 to obtain a highly active binder;

[0096] 3) mixing nano zirconium oxide powder and nano titanium carbonitride powder in a mass ratio of 1:2.5 to obtain a nano additive;

[0097] 4) using a planetary ball mill, anhydrous ethanol as the ball milling medium, equipped with a stainless steel ball mill and a high-hardness metal ball mill, the basic hardness aggregate is wet-milled at a ball milling speed of 65 r / min for 50 h; the milled material is transferred to a V-type mixer, a high-activity binder of 12% of the mass of the basic hardness aggregate is added and stirred at 58 r / min for 1 h, and then a nano-additive of 2.5% of the mass of the basic hardness aggregate is added and stirred at 95 r / min for 6 h; the stirred material is introduced into a glass container, and an ultrasonic device is used to disperse it for 25 min to obtain a mixed slurry;

[0098] 5) After the mixed slurry is dried, it is passed through a 320-mesh sieve, and the sieve-underground material is taken out and then subjected to vacuum hot isostatic pressing sintering with a vacuum degree of 4×10 -3 Pa, sintering temperature is 1450℃, sintering pressure is 25MPa, holding time is 3h, the sintered product is crushed to obtain nanocomposite coating powder with a particle size of 6μm;

[0099] 6) The surface of the copper plate substrate of the crystallizer is treated, the rust removal grade is St3, and the roughness reaches 3 μmRa. The nano-composite coating powder is sprayed onto the surface of the copper plate substrate of the crystallizer by supersonic flame spraying to form a nano-composite coating with a thickness of 2.8 mm.

[0100] After testing, the density of the nano-composite coating prepared in this embodiment is 99.9%, the hardness HV reaches 750, the bonding strength between the nano-composite coating and the crystallizer copper plate substrate is 385 MPa, and the actual single-time steel passing capacity of the crystallizer copper plate with the nano-composite coating is 145,000 tons / set, and the service life is 3,400 furnaces.

[0101] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. A method for preparing a nano-composite coating on the surface of a crystallizer copper plate, characterized in that: The following steps are involved: 1) Premix tungsten carbide powder, tungsten powder and titanium carbide powder to obtain basic hardness aggregate; 2) premixing cobalt powder, carbonyl iron powder and carbonyl nickel powder to obtain a highly active binder; 3) Premixing nano zirconium oxide powder and nano titanium carbonitride powder to obtain a nano additive; 4) wet-milling the basic hardness aggregate, then adding a high-activity binder for primary stirring, then adding a nano-additive for secondary stirring, and finally performing ultrasonic dispersion to obtain a mixed slurry; 5) drying the mixed slurry and sieving it, and then sintering it by vacuum hot pressing or vacuum hot isostatic pressing, crushing the sintered product to obtain a nanocomposite coating powder; 6) The surface of the copper plate substrate of the crystallizer is treated to make the rust removal and roughness meet the spraying requirements, and the nano-composite coating powder is sprayed onto the surface of the copper plate substrate of the crystallizer by supersonic flame spraying or plasma spraying to form a nano-composite coating.

2. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: In the basic hardness aggregate, the particle size of tungsten carbide powder is less than 3 μm, the particle size of tungsten powder is less than 1 μm, and the particle size of titanium carbide powder is less than 1 μm. The mass ratio of tungsten carbide powder, tungsten powder and titanium carbide powder is (4-6):(1-2):

1.

3. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: In the highly active binder, the particle size of the cobalt powder is less than 1 μm, the particle size of the carbonyl iron powder is less than 2 μm, the particle size of the carbonyl nickel powder is less than 2 μm, and the mass ratio of the cobalt powder, the carbonyl iron powder and the carbonyl nickel powder is 1:(1-3):(1-3).

4. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: In the nano additive, the particle size of the nano zirconium oxide powder is 20-60 nm, the particle size of the nano titanium carbonitride powder is 50-200 nm, and the mass ratio of the nano zirconium oxide powder to the nano titanium carbonitride powder is 1:(2-4).

5. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: The mass of the high-activity binder is 10-20% of the mass of the basic hardness aggregate, and the mass of the nano additive is 1-5% of the mass of the basic hardness aggregate.

6. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: The wet ball milling adopts a planetary ball mill, anhydrous ethanol as the ball milling medium, a stainless steel ball milling jar and a high-hardness metal ball mill, a ball milling speed of 50-100 r / min, and a ball milling time of 30-60 hours.

7. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: The stirring is performed using a V-type mixer; the stirring rate of the first stirring is 50-60 r / min, and the stirring time is 0.5-1 h; the stirring rate of the second stirring is 80-10 r / min, and the stirring time is 4.5-9 h.

8. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: The vacuum degree of the vacuum hot pressing sintering or vacuum hot isostatic pressing sintering is 3.5×10 -3 ~4.5×10 -3 Pa, the sintering temperature is 1400-1500℃, the pressure is 20-40MPa, and the holding time is 1-3h.

9. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: The particle size of the nano-composite coating powder is less than 10 μm; the crystallizer copper plate substrate is Ag-Cu alloy or Cu-Cr-Zr alloy; the rust removal grade of the crystallizer copper plate substrate is Sa3, St2 or St3, and the roughness should reach 2.5-5 μmRa.

10. The method for preparing a nano-composite coating on a surface of a crystallizer copper plate according to claim 1, characterized in that: The thickness of the nano-composite coating is 1.5-3 mm, the density is greater than 99.7%, the hardness HV is 500-800, the bonding strength between the nano-composite coating and the crystallizer copper plate substrate is 200-400 MPa, the crystallizer copper plate with the nano-composite coating has a single steel passing capacity of 80,000-150,000 tons / set, and a service life of 2,800-3,500 furnaces.

Citation Information

Patent Citations

  • Thermal spraying powder for preparing superhigh pressure sealing coating and preparation process thereof

    CN102586712A

  • Preparation method for continuous casting mold long-edge copper plate composite coating

    CN109576628A

  • Preparation method of metal element Ti / Cr and hard phase WC in-situ codoped nanocrystalline tungsten-copper-based composite material

    CN109837442A

  • Coating composite material, preparation method of coating composite material, coating, crystallizer copper plate and surface treatment method of crystallizer copper plate

    CN114940837A

  • Preparation method of coating for crystallizer copper plate

    CN115110018A