Water-based antirust primer with high corrosion resistance and salt spray resistance
By adding water-based modified isocyanosilane additives to the water-based anti-rust primer, the problem of poor adhesion and salt spray resistance during the coating process is solved, and high adhesion and salt spray resistance are improved. , suitable for automotive metal products and is environmentally friendly.
Patent Information
- Application Number
- CN202411427913.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-12-06
AI Technical Summary
During the coating process of existing steel protective materials, the surface rust removal treatment is complicated and the coating adhesion is poor. The salt spray resistance of high corrosion-resistant water-resistant anti-rust primer is poor, and it cannot meet the standards of oily anti-rust primer. Water-based coatings need to improve adhesion and water resistance.
By adding water-based modified isocyanisilane additives, the degree of cross-linking of the coating is enhanced, the coating adhesion is improved, and specific component ratios and process steps are adopted, including premixing and paint making steps, to improve the salt spray and water resistance of the coating. sex.
It significantly improves the adhesion and salt spray resistance of the substrate coating, meets the coating process requirements of automotive metal products, and does not contain benzene solvents. It is environmentally friendly and suitable for industrial production.
Smart Images

Figure FT_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coating preparation, and particularly relates to a highly corrosion-resistant and salt-spray-resistant water-based rust-proof primer. Background Art
[0002] At present, the widely used steel protective materials often require a more thorough surface rust removal treatment of the metal substrate before painting to achieve the necessary coating adhesion strength; while the existing rust-bearing coatings are mainly phosphoric acid and organic acid, which can only oxidize the surface of the rust layer, but cannot penetrate into the interior, and the paint film is prone to blistering, loosening or falling off. At the same time, the corrosion resistance and salt spray resistance of the highly corrosion-resistant water-based anti-rust primer widely used in the existing automotive coatings industry are not very ideal, basically around 100 hours, far from the requirements of 500-1000 hours of corrosion resistance and salt spray resistance of oil-based anti-rust primers. In addition, with the enhancement of environmental awareness in recent years, water-based coatings have been vigorously promoted. They do not add any solvents such as benzene, are quite friendly to the environment, and only need to be cleaned with water after construction, saving a lot of costs, but water-based epoxy is directly in contact with the coating as the substrate, and its adhesion, water resistance and salt spray resistance are the top priority. Summary of the invention
[0003] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a highly corrosion-resistant and salt-spray-resistant water-based anti-rust primer, which enhances the degree of cross-linking by adding a water-based modified isocyanosilane additive, and can improve the workability of the material, greatly improve the adhesion of the substrate coating, and thus greatly improve the salt spray resistance and water resistance.
[0004] To achieve the above object, the present invention adopts the following technical solution: A highly corrosion-resistant and salt-spray-resistant water-based antirust primer, comprising the following components in parts by weight: 40 parts of waterborne epoxy resin; Pigment 15 parts; 28 parts of filler; 10 parts of deionized water; 5-7 parts of water-based additives; 0.1 part of water-based modified isocyanosilane additive; The water-based additive consists of a water-based anti-settling agent, a water-based dispersant, a water-based leveling agent, a water-based anti-flash rust agent, a water-based defoaming agent, a water-based thixotropic agent, a water-based thickener, and a film-forming additive.
[0005] Furthermore, the pigment is one or more of titanium dioxide and carbon black.
[0006] Furthermore, the filler is one or more of precipitated barium sulfate, talcum powder, zinc phosphomolybdate, zinc phosphate, and aluminum tripolyphosphate.
[0007] Furthermore, the mass ratio of the water-based anti-settling agent, water-based dispersant, water-based leveling agent, water-based anti-flash rust agent, water-based defoaming agent, water-based thixotropic agent, water-based thickener and film-forming aid in the water-based additive is 0.3:1:0.2:1:0.2:0.1:1:3.
[0008] Furthermore, the water-based modified isocyanate silane auxiliary agent is prepared by reacting isocyanate and epoxy silane in a mass ratio of 1:1, and the reaction formula is: ; Specifically, isocyanate is dissolved and diluted with propylene glycol diacetate (PGDA) to form a 30wt% solution, and then epoxy silane is added, and the reaction is stirred at 80°C and 800r / min for 30min, and the solution is cooled to a slightly yellow transparent solution and then allowed to stand for 3h, and then filtered under reduced pressure to remove impurities, thereby obtaining the water-based modified isocyanosilane auxiliary agent.
[0009] The use of the water-based modified isocyanosilane additive can improve the cross-linking property of the coating and enhance the adhesion of the coating, thereby improving the salt spray resistance and water resistance of the base coating and improving the storage stability of the coating.
[0010] The preparation method of the highly corrosion-resistant and salt-spray-resistant water-based antirust primer comprises the following steps: (1) Premixing: Slowly add aqueous dispersant, aqueous defoamer, aqueous anti-settling agent, pigment and filler to deionized water in sequence, stir at high speed for 30-60 minutes, and then grind to a slurry fineness of ≤25μm; (2) Paint preparation: Add a water-based leveling agent, a water-based thixotropic agent, a water-based epoxy resin, a water-based thickener, a film-forming aid, a water-based flash rust inhibitor and a water-based modified isocyanosilane additive to the slurry obtained in step (1), stir for 30-40 minutes and then filter to obtain the highly corrosion-resistant and salt-spray-resistant water-based anti-rust primer.
[0011] Furthermore, the speed of the high-speed stirring in step (1) is 800-1000 r / min.
[0012] Furthermore, the stirring speed in step (3) is 600-800 r / min.
[0013] The highly corrosion-resistant and salt-spray-resistant water-based antirust primer prepared by the present invention can be used as a primer for metal products and the like for coating to achieve the effects of corrosion resistance and salt-spray resistance. The specific operation is as follows: (1) Spraying: Spray the highly corrosion-resistant and salt-spray-resistant water-based anti-rust primer on metal products and allow it to flow for 10-15 minutes; (2) Drying: Bake the sprayed product at 70-80℃ for 45-60min, then cool to room temperature and leave for 24-72 hours.
[0014] The beneficial effects of the present invention are: The highly corrosion-resistant and salt-spray-resistant water-based antirust primer prepared by the present invention has excellent performance, and its performance meets the coating process requirements of automobile metal products: First, it has better adhesion and meets the salt spray resistance standard (more than 500h) compared with ordinary epoxy products; Second, the impact performance is excellent; Third, it does not contain harmful solvents such as benzene and is environmentally friendly; Fourth, it can be implemented on the basis of existing equipment, and its preparation process is simple and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the infrared spectrum of the prepared coating. DETAILED DESCRIPTION
[0016] A highly corrosion-resistant and salt-spray-resistant water-based antirust primer, comprising the following components in parts by weight: 40 parts of waterborne epoxy resin; Pigment 15 parts; 28 parts of filler; 10 parts of deionized water; 5-7 parts of water-based additives; 0.1 part of water-based modified isocyanosilane additive.
[0017] Wherein, the pigment is one or more of titanium dioxide and carbon black.
[0018] The filler is one or more of precipitated barium sulfate, talcum powder, zinc phosphomolybdate, zinc phosphate, and aluminum tripolyphosphate.
[0019] The water-based additive is composed of a water-based anti-settling agent, a water-based dispersant, a water-based leveling agent, a water-based anti-flash rust agent, a water-based defoaming agent, a water-based thixotropic agent, a water-based thickener, and a film-forming additive in a mass ratio of 0.3:1:0.2:1:0.2:0.1:1:3.
[0020] The water-based modified isocyanate silane auxiliary agent is prepared by dissolving isocyanate with propylene glycol diacetate (PGDA) to dilute it into a 30wt% solution, then adding epoxy silane, stirring and reacting for 30min at 80°C and a rotation speed of 800r / min, cooling it to a slightly yellow transparent solution and then standing it for 3h, and then filtering it under reduced pressure to remove impurities, wherein the mass ratio of isocyanate to epoxy silane is 1:1.
[0021] The preparation method of the highly corrosion-resistant and salt-spray-resistant water-based antirust primer comprises the following steps: (1) Premixing: Slowly add aqueous dispersant, aqueous defoamer, aqueous anti-settling agent, pigment and filler into deionized water in sequence, stir at 800-1000r / min for 30-60min, and then grind to a slurry fineness of ≤25μm; (2) Paint preparation: Add a water-based leveling agent, a water-based thixotropic agent, a water-based epoxy resin, a water-based thickener, a film-forming aid, a water-based flash rust inhibitor and a water-based modified isocyanosilane aid to the slurry obtained in step (1), stir at 600-800 r / min for 30-40 min, and then filter to obtain the slurry.
[0022] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0023] In the case of illustrating and explaining the purpose of the present invention through the following examples, the components of the composition are explained in parts by weight as a general standard. Unless otherwise specified, for the sake of simplicity, the "parts" described in the examples of the present invention have the same meaning as parts by weight.
[0024] Specific raw material description: Water-based epoxy resin: 3012 was purchased from Fuqisen Company; Pigment: MA100 carbon black is purchased from Mitsubishi Corporation of Japan. Titanium dioxide was purchased from Billions-Longmang Company’s R996; Filler: Composite zinc phosphate was purchased from Shanghai Junjiang Chemical Co., Ltd. Precipitated barium sulfate was purchased from Shanghai Junjiang Chemical Co., Ltd. 1250 mesh talc powder was purchased from Shanghai Junjiang Chemical Co., Ltd.; Water-based anti-settling agent: R972 purchased from Degussa; Water-based dispersant: BYK190 was purchased from BYK Chemical Company of Germany; Water-based leveling agent: 4100 purchased from Digao Chemical; Water-based flash rust preventer: H10 is purchased from Hemmings Deqian; Water-based defoamer: 902W was purchased from Digo Chemical Company; Water-based thixotropic agent: XS83 purchased from Hemmingsdeqian; Water-based thickener: 30% HV30 purchased from Guangdong Huaguoshan Chemical Co., Ltd.; Film-forming aid: purchased from Hemmingsdeqian.
[0025] The aqueous modified isocyanate silane additive was prepared by the laboratory. The preparation method was to dissolve isocyanate with PGDA to dilute it into a 30wt% solution, then add epoxy silane, stir and react for 30min at 80°C and 800r / min, cool to a slightly yellow transparent solution and let stand for 3h, then filter under reduced pressure to obtain the product, wherein the mass ratio of isocyanate to epoxy silane was 1:1.
[0026] Example 1 Table 1 Formula of anti-rust primer
[0027] The preparation of highly corrosion-resistant and salt-spray-resistant water-based anti-rust primer includes the following steps: (1) Premixing: According to the formula in Table 1, add deionized water into the dispersion tank and stir; then slowly add dispersant, defoamer, anti-settling agent, pigment and filler in sequence, and stir at a high speed of 1000r / min for 30 min; (2) Grinding: Grind the premixed slurry with a sand mill to a fineness of ≤25 μm; (3) Paint making: Add leveling agent, water-based modified isocyanate silane additive, water-based epoxy resin, water-based thickener, film-forming additive, water-based anti-flash rust agent and water-based thixotropic agent to the ground slurry, stir at 800 r / min for 30 min, and filter to obtain the paint.
[0028] Example 2 The dosage of the water-based modified isocyanosilane auxiliary agent was changed to 0.2 parts, and the other operations were the same as in Example 1.
[0029] Example 3 The dosage of the water-based modified isocyanosilane auxiliary agent was changed to 0.3 parts, and the other operations were the same as in Example 1.
[0030] Comparative Example 1 Except that the water-based modified isocyanosilane auxiliary agent is not used, other operations are the same as those in Example 1.
[0031] Comparative Example 2 Epoxy silane was used instead of the water-based modified isocyanosilane auxiliary agent, and other operations were the same as in Example 1.
[0032] Performance Testing The method and detection method of water-based anti-rust primer for automobile painting are as follows: Ⅰ. Prepare the matching curing agent according to the formula in Table 2, then prepare the primer and curing agent according to the weight ratio of 10:1, and then adjust the viscosity to 25-30S with deionized water, spray it on the polished automotive galvanized sheet and cold-rolled sheet (spraying pressure 0.4MPa, control the film thickness at 50-60μm), and level it for 10-15min; Ⅱ. Bake the sprayed metal plate at 70-80℃ for 40 minutes. After cooling, test the adhesion, flexibility and impact according to the method in Table 3. After standing for 72 hours, test the water resistance, salt spray resistance, acid and alkali resistance and gasoline resistance.
[0033] Table 2 Formula of supporting curing agent
[0034] Table 3 Performance testing methods
[0035] Table 4 Comparison of test results of various embodiments
[0036] From the results in Table 4, it can be seen that adding excessive modified isocyanosilane additives will deteriorate the salt spray resistance and water resistance of the obtained water-based anti-rust primer. Therefore, adding 0.1 parts of modified isocyanosilane additives is the best effect.
[0037] Table 5 Comparison of test results of Example 1 and Comparative Example
[0038] It can be seen from Table 5 that the water-based anti-rust primer prepared without adding water-based modified isocyanate silane additives or directly using epoxy silane will have deviations in adhesion when not polished, and its salt spray resistance is far from the requirement of more than 500h for oily products; while the performance of the water-based anti-rust primer prepared with the addition of water-based modified isocyanate silane additives meets the coating process requirements of automotive metal products: that is, after baking at 70-80℃×40min, the adhesion is level 0, the salt spray resistance is 1200h, and the water resistance is 1200h.
[0039] Obviously, the above embodiments of the present invention are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description, and all changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention. All documents mentioned in the present invention are cited as references in this application, just as a document is cited as a reference alone.
Claims
1. A highly corrosion-resistant and salt-spray-resistant water-based anti-rust primer, characterized in that: The water-based anti-rust primer includes the following components by weight: 40 parts of waterborne epoxy resin; Pigment 15 parts; 28 parts of filler; 10 parts of deionized water; 5-7 parts of water-based additives; 0.1 part of water-based modified isocyanosilane additive; The water-based auxiliary agent consists of a water-based anti-settling agent, a water-based dispersant, a water-based leveling agent, a water-based anti-flash rust agent, a water-based defoaming agent, a water-based thixotropic agent, a water-based thickener and a film-forming auxiliary agent.
2. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 1, characterized in that: The pigment is one or more of titanium dioxide and carbon black.
3. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 1, characterized in that: The filler is one or more of precipitated barium sulfate, talcum powder, zinc phosphomolybdate, zinc phosphate, and aluminum tripolyphosphate.
4. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 1, characterized in that: The mass ratio of the water-based anti-settling agent, water-based dispersant, water-based leveling agent, water-based flash rust preventer, water-based defoamer, water-based thixotropic agent, water-based thickener and film-forming aid in the water-based additive is 0.3:1:0.2:1:0.2:0.1:1:
3.
5. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 1, characterized in that: The water-based modified isocyanate auxiliary agent is prepared by dissolving isocyanate with propylene glycol diacetate to dilute it into a 30wt% solution, then adding epoxy silane, stirring and reacting for 30min at 80°C and 800r / min, cooling to a slightly yellow transparent solution, standing for 3h, and then filtering under reduced pressure.
6. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 5, characterized in that: The mass ratio of isocyanate to epoxy silane used is 1:
1.
7. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 1, characterized in that: The preparation method comprises the following steps: (1) Premixing: Slowly add aqueous dispersant, aqueous defoamer, aqueous anti-settling agent, pigment and filler to deionized water in sequence, stir at high speed for 30-60 minutes, and then grind to a slurry fineness of ≤25μm; (2) Paint preparation: Add a water-based leveling agent, a water-based thixotropic agent, a water-based epoxy resin, a water-based thickener, a film-forming aid, a water-based flash rust inhibitor and a water-based modified isocyanosilane additive to the slurry obtained in step (1), stir for 30-40 minutes and then filter to obtain the highly corrosion-resistant and salt-spray-resistant water-based anti-rust primer.
8. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 7, characterized in that: The speed of the high-speed stirring in step (1) is 800-1000 r / min.
9. The highly corrosion-resistant and salt-spray-resistant water-based antirust primer according to claim 7, characterized in that: The stirring speed in step (3) is 600-800 r / min.
Citation Information
Patent Citations
Epoxy silane oligomer and coating composition containing same
CN101365763A
Water-based epoxy anticorrosive paint with long-acting resistance to acid and alkali corrosion and preparation method thereof
CN110894391A
Salt-spray-resistant coiled material household appliance primer
CN111534191A
Water-based two-component anticorrosive paint
CN114958187A
Silane modified epoxy waterborne polyurethane steel structure anticorrosive paint
CN115260890A