Adhesive film

By adopting a double-layer structure in the adhesive film, using the combination of dendrite conductive particles and non-conductive nucleobody conductive layer, the problem of insufficient conductivity and reliability of existing adhesives in electronic components is solved, and the problem of insufficient conductivity and reliability of existing adhesives in the connection of electronic components is realized. It has high reliability and heat resistance, and is suitable for high-density applications such as liquid crystal displays.

CN119081562APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201635.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2017-02-17
Filing Date
2018-02-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing adhesives are inadequate in conductivity and reliability in fixing and circuit connections of electronic components, especially in liquid crystal displays and other high-density, high-refining applications, which are difficult to meet performance requirements.

Method used

Adhesive film with a double-layer structure, wherein the first layer contains dendrite conductive particles and the second layer contains a conductive layer arranged on a non-conductive nucleus. The volume ratio of the conductive particles of the second layer is greater than that of the first layer, and the use is free Materials such as gold, nickel and palladium form conductive layers, improving conductivity and fluidity to enhance adhesion and reliability.

Benefits of technology

High reliability and conductivity under ambient temperature changes are achieved, electronic components of different materials can be effectively connected, heat and moisture resistance of the adhesive, and adhesive strength and connection stability are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081562A_ABST
    Figure CN119081562A_ABST
Patent Text Reader

Abstract

The invention relates to an adhesive film. This adhesive film is provided with a first adhesive layer and a second adhesive layer, and the first adhesive layer contains: a first adhesive component; a first conductive particle that is a dendritic conductive particle; and second conductive particles that are conductive particles other than the first conductive particles and that have a non-conductive core and a conductive layer provided on the core, the second adhesive layer containing a second adhesive component. The volume ratio of the second adhesive component in the second adhesive layer is greater than the volume ratio of the first adhesive component in the first adhesive layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of the invention application with application number 201880011884.7 (international application number PCT / JP2018 / 005033), application date February 14, 2018, and invention name “Adhesive Film”. Technical Field

[0002] The present invention relates to an adhesive film. Background Art

[0003] In recent years, various adhesives have been used in the fields of semiconductors, liquid crystal displays, etc. for fixing electronic components, connecting circuits, etc. In these applications, the density and precision of electronic components, circuits, etc. are constantly advancing, and thus adhesives are also required to have higher levels of performance.

[0004] For example, in the connection between a liquid crystal display and a TCP (Tape Carrier Package), a connection between an FPC (Flexible Printed Circuit) and a TCP, or a connection between an FPC and a printed wiring board, an adhesive in which conductive particles are dispersed is used. Such an adhesive is required to further improve conductivity and reliability.

[0005] For example, Patent Document 1 describes a conductive film having a conductive film containing predetermined dendritic silver-coated copper powder particles on a base film, and discloses that sufficient conductive properties can be obtained with this conductive film even without adding silver powder.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: International Publication No. 2014 / 021037 Summary of the invention

[0009] Problems to be solved by the invention

[0010] An object of the present invention is to provide an adhesive film having excellent reliability.

[0011] Solution to the problem

[0012] One aspect of the present invention is an adhesive film comprising a first adhesive layer and a second adhesive layer, wherein the first adhesive layer contains: a first adhesive component; first conductive particles, which are dendrite-shaped conductive particles; and second conductive particles, which are conductive particles other than the first conductive particles and are conductive particles having a non-conductive core and a conductive layer disposed on the core, wherein the second adhesive layer contains a second adhesive component, and the volume ratio of the second adhesive component in the second adhesive layer is greater than the volume ratio of the first adhesive component in the first adhesive layer.

[0013] The second adhesive layer may contain only the second adhesive component.

[0014] The conductive layer may contain at least one selected from the group consisting of gold, nickel, and palladium.

[0015] Effects of the Invention

[0016] According to the present invention, an adhesive film having excellent reliability can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a schematic cross-sectional view showing one embodiment of the adhesive film.

[0018] Figure 2 This is a cross-sectional view of main parts schematically showing an example of connection between electronic components.

[0019] Figure 3 It is a schematic diagram showing a method of manufacturing a mounting body for reliability testing.

[0020] Figure 4 This is a schematic diagram showing a mounting body for reliability testing.

[0021] Figure 5 This is a schematic diagram showing a method for measuring connection resistance in a reliability test.

[0022] Explanation of symbols

[0023] 1: adhesive film, 2: first adhesive layer, 3: second adhesive layer, 4: first adhesive component, 5: first conductive particles, 6: second conductive particles, 7: second adhesive component. DETAILED DESCRIPTION

[0024] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings as appropriate.

[0025] Figure 1 Schematic cross-sectional view showing one embodiment of an adhesive film. Figure 1As shown, the adhesive film 1 includes a first adhesive layer 2 and a second adhesive layer 3. The first adhesive layer 2 contains a first adhesive component 4, and first conductive particles 5 and second conductive particles 6 dispersed in the first adhesive component 4. The second adhesive layer 3 contains a second adhesive component 7.

[0026] The first adhesive component 4 and the second adhesive component 7 may be of the same type or different types, but are preferably of the same type from the viewpoint of obtaining a stable adhesive force against changes in ambient temperature. The first adhesive component 4 and the second adhesive component 7 may be adhesive components described below.

[0027] As the adhesive component, for example, it is composed of a material that shows curability by heat or light, and can be an epoxy adhesive, a free radical curing adhesive, a thermoplastic adhesive such as polyurethane, polyvinyl ester, etc. From the perspective of excellent heat resistance and moisture resistance after bonding, the adhesive component can also be composed of a cross-linking material. Among them, from the perspectives of being able to cure in a short time and having good connection workability and excellent adhesion, it is preferred to use an epoxy adhesive containing an epoxy resin belonging to a thermosetting resin as the main component. Free radical curing adhesives have the characteristics of excellent curability in a short time at low temperature compared to epoxy adhesives, so they can be used appropriately according to the purpose.

[0028] The epoxy adhesive contains, for example, a thermosetting material such as an epoxy resin and a curing agent, and may further contain a thermoplastic resin, a coupling agent, a filler, and the like as necessary.

[0029] As epoxy resin, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, alicyclic epoxy resin, glycidyl ester type epoxy resin, glycidylamine type epoxy resin, hydantoin type epoxy resin, isocyanurate type epoxy resin, aliphatic chain epoxy resin, etc. can be listed. These epoxy resins can be halogenated or hydrogenated, and can also have a structure with an acryloyl group or a methacryloyl group added to the side chain. These epoxy resins can be used alone or in combination of two or more.

[0030] The curing agent is not particularly limited as long as it can cure the epoxy resin, and examples thereof include anionic polymerization catalyst-type curing agents, cationic polymerization catalyst-type curing agents, addition polymerization-type curing agents, etc. The curing agent is preferably anionic or cationic polymerization catalyst-type curing agents because of excellent rapid curing properties and no need to consider chemical equivalents.

[0031] Anionic or cationic polymerization catalyst-type curing agents may be, for example, imidazole-based, hydrazide-based, boron trifluoride-amine complex, Salts (aromatic sulfonium salts, aromatic diazo Onium salts, aliphatic sulfonium salts, etc.), amine imide, diamino maleic dinitrile, melamine and its derivatives, salts of polyamines, dicyandiamide, etc., and their modified products may also be used. Examples of polyaddition type curing agents include polyamines, polymercaptans, polyphenols, acid anhydrides, etc.

[0032] Latent curing agents that are coated and microencapsulated with high molecular weight materials such as polyurethane and polyester, metal films such as nickel and copper, and inorganic materials such as calcium silicate are preferred because they can extend the service life. The curing agents can be used alone or in combination of two or more.

[0033] The content of the curing agent may be 0.05 to 20 parts by mass relative to 100 parts by mass of the total amount of the thermosetting material and the thermoplastic resin blended as required.

[0034] The radical curing adhesive contains, for example, a radical polymerizable material and a radical polymerization initiator (also referred to as a curing agent), and may further contain a thermoplastic resin, a coupling agent, a filler, and the like as necessary.

[0035] As a free radical polymerizable material, for example, any material having a functional group that is polymerized by free radicals can be used without particular limitation. Specifically, the free radical polymerizable material may be, for example, free radical polymerizable substances such as acrylate (including corresponding methacrylate. The same applies hereinafter.) compounds, acryloxy (including corresponding methacryloyloxy. The same applies hereinafter.) compounds, maleimide compounds, citraconimide resins, and nadicimide resins. These free radical polymerizable substances may be in the form of monomers or oligomers, or in the form of a mixture of monomers and oligomers.

[0036] Examples of the acrylate compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, isobutyl acrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, 2-hydroxy-1,3-diacryloxypropane, 2,2-bis[4-(acryloxymethoxy)phenyl]propane, 2,2-bis[4-(acryloxypolyethoxy)phenyl]propane, dicyclopentenyl acrylate, tricyclodecyl acrylate, tris(acryloxyethyl)isocyanurate, urethane acrylate, and phosphate diacrylate.

[0037] Free radical polymerizable substances such as acrylate compounds can also be used together with inhibitors such as hydroquinone and methyl ether hydroquinone as needed. From the viewpoint of improving heat resistance, free radical polymerizable substances such as acrylate compounds preferably have at least one substituent such as dicyclopentenyl, tricyclodecyl, triazine ring, etc. As free radical polymerizable substances other than acrylate compounds, for example, compounds described in International Publication No. 2009 / 063827 can be used appropriately. Free radical polymerizable substances can be used alone or in combination of two or more.

[0038] As a free radical polymerization initiator, as long as it is a compound that decomposes and generates free radicals by heating or light irradiation, it can be used without particular limitation. Specifically, the free radical polymerization initiator can be, for example, a peroxide compound, an azo compound, etc. These compounds can be appropriately selected according to the target connection temperature, connection time, effective time, etc.

[0039] Radical polymerization initiator is more specifically preferably diacyl peroxide, peroxydicarbonate, peroxyester, peroxyketal, dialkyl peroxide, hydrogen peroxide, silyl peroxide etc.Wherein, be peroxyester, dialkyl peroxide, hydrogen peroxide, silyl peroxide etc., from the viewpoint that can obtain high reactivity, more preferably peroxyester.As these radical polymerization initiators, for example, can suitably use the compound of putting down in writing in International Publication No. 2009 / 063827.Radical polymerization initiator can use one kind alone or use two or more in combination.

[0040] The content of the radical polymerization initiator may be 0.1 to 10 parts by mass based on 100 parts by mass of the total amount of the radical polymerizable material and the thermoplastic resin blended as required.

[0041] Thermoplastic resins that are matched as needed in epoxy adhesives and free radical curing adhesives are, for example, easy to give excellent film formability to the adhesive. As thermoplastic resins, for example, phenoxy resins, polyvinyl formal resins, polystyrene resins, polyvinyl butyral resins, polyester resins, polyamide resins, xylene resins, polyurethane resins, polyester urethane resins, phenolic resins, terpene phenolic resins, etc. can be cited. As thermoplastic resins, for example, compounds described in International Publication No. 2009 / 063827 can be used appropriately. From the aspects of excellent adhesion, compatibility, heat resistance, mechanical strength, etc., thermoplastic resins are preferably phenoxy resins. Thermoplastic resins can be used alone or in combination of two or more.

[0042] The content of the thermoplastic resin, when mixed with an epoxy adhesive, can be 5 to 80 parts by mass relative to 100 parts by mass of the total amount of the thermoplastic resin and the thermosetting material. The content of the thermoplastic resin, when mixed with a radical curing adhesive, can be 5 to 80 parts by mass relative to 100 parts by mass of the total amount of the thermoplastic resin and the radical polymerizable material.

[0043] As another example of the adhesive component, a thermal radical curing adhesive can be cited, which contains a thermoplastic resin, a radical polymerizable material containing a radical polymerizable substance that is liquid at 30°C, and a radical polymerization initiator. The thermal radical curing adhesive has a lower viscosity than the above-mentioned adhesive components. The content of the radical polymerizable substance in the thermal radical curing adhesive is preferably 20 to 80 parts by mass, more preferably 30 to 80 parts by mass, and further preferably 40 to 80 parts by mass, relative to 100 parts by mass of the total amount of the thermoplastic resin and the radical polymerizable substance.

[0044] The adhesive component may also be an epoxy adhesive containing a thermoplastic resin, a thermosetting material containing an epoxy resin that is liquid at 30° C., and a curing agent. In this case, the content of the epoxy resin in the epoxy adhesive is preferably 20 to 80 parts by mass, more preferably 40 to 80 parts by mass, and further preferably 30 to 80 parts by mass, relative to 100 parts by mass of the total amount of the thermoplastic resin and the thermosetting material.

[0045] In the case where the adhesive film 1 is used for the connection between an IC chip and a glass substrate, a flexible printed circuit board (FPC), etc., from the viewpoint of suppressing the warping of the substrate caused by the difference in the linear expansion coefficient of the IC chip and the substrate, the adhesive composition preferably further contains a component that plays a role in relieving internal stress. As the above-mentioned component, specifically, acrylic rubber, elastomeric components, etc. can be cited. Alternatively, the adhesive composition can also be a free radical curing adhesive as described in International Publication No. 98 / 44067.

[0046] Based on the total volume of the first adhesive layer 2, the volume ratio of the first adhesive component 4 in the first adhesive layer 2 can be, for example, greater than or equal to 55 volume % or greater than or equal to 65 volume %, and can be less than or equal to 95 volume % or less than or equal to 85 volume %.

[0047] The first conductive particles 5 are dendritic (also called branched) and have a main axis and a plurality of branches branching from the main axis two-dimensionally or three-dimensionally. The first conductive particles 5 can be made of metal such as copper and silver, for example, silver-coated copper particles.

[0048] The first conductive particles 5 may be known conductive particles, and specifically, may be obtained as ACBY-2 (Mitsui Mining & Smelting Co., Ltd.) or CE-1110 (Fukuda Metal Foil Co., Ltd.) Alternatively, the first conductive particles 5 may be produced by a known method (for example, the method described in Patent Document 1).

[0049] Based on the total volume of the first adhesive layer 2, the content of the first conductive particles 5 in the first adhesive layer 2 (the volume proportion of the first conductive particles 5 in the first adhesive layer 2) can be greater than or equal to 2 volume % or greater than or equal to 8 volume %, and can be less than or equal to 25 volume % or less than or equal to 15 volume %.

[0050] The second conductive particles 6 have a non-conductive core and a conductive layer disposed on the core. The core is formed of a non-conductive material such as glass, ceramic, or resin, preferably a resin. Examples of the resin include acrylic resin, styrene resin, silicone resin, polybutadiene resin, or copolymers of monomers constituting these resins. The average particle size of the core may be, for example, 2 to 30 μm.

[0051] The conductive layer is formed of, for example, gold, silver, copper, nickel, palladium or an alloy thereof. From the viewpoint of excellent conductivity, the conductive layer preferably contains at least one selected from gold, nickel and palladium, more preferably contains gold or palladium, and further preferably contains gold. The conductive layer is formed, for example, by plating the above metals on the core. The thickness of the conductive layer can be, for example, 10 to 400 nm.

[0052] From the viewpoint of being able to appropriately thin the film, the average particle size of the second conductive particles 6 is preferably less than or equal to 30 μm, more preferably less than or equal to 25 μm, and further preferably less than or equal to 20 μm. The average particle size of the second conductive particles 6 can be, for example, greater than or equal to 1 μm. The average particle size of the second conductive particles 6 is measured by a particle size distribution measuring device (Microtrac (product name, Nikkiso Co., Ltd.)) using a laser diffraction scattering method.

[0053] Based on the total volume of the first adhesive layer 2, the content of the second conductive particles 6 in the first adhesive layer 2 (the volume proportion of the second conductive particles 6 in the first adhesive layer 2) can be greater than or equal to 2 volume % or greater than or equal to 5 volume %, and can be less than or equal to 20 volume % or less than or equal to 10 volume %.

[0054] The thickness of the first adhesive layer 2 may be, for example, 5 μm or more, 7 μm or more, or 10 μm or more, and may be 30 μm or less, 25 μm or less, or 20 μm or less.

[0055] The second adhesive layer 3 contains a second adhesive component 7. The thickness of the second adhesive layer 3 may be, for example, 5 μm or more, 7 μm or more, or 10 μm or more, and 30 μm or less, 25 μm or less, or 20 μm or less.

[0056] In the above-described embodiment, the second adhesive layer 3 contains only the second adhesive component 7 , but the second adhesive layer may further contain conductive particles such as the first conductive particles 5 and the second conductive particles 6 .

[0057] In the case where the second adhesive layer further contains conductive particles, from the viewpoint of appropriately filling the unevenness when the surface of the electronic component has unevenness, the volume ratio of the second adhesive component 7 in the second adhesive layer is greater than the volume ratio of the first adhesive component 4 in the first adhesive layer 2. Based on the total volume of the second adhesive layer, the volume ratio of the second adhesive component 7 in the second adhesive layer can be, for example, greater than or equal to 90 volume%, greater than or equal to 95 volume%, or greater than or equal to 98 volume%. In addition, from the same viewpoint, the second adhesive layer preferably contains only the second adhesive component 7 as in the above embodiment.

[0058] The adhesive film 1 is obtained, for example, by forming the first adhesive layer 2 and the second adhesive layer 3 separately and then laminating them. The first adhesive layer 2 and the second adhesive layer 3 are obtained, for example, by applying a paste adhesive composition on a resin film such as a PET (polyethylene terephthalate) film and drying them. The paste adhesive composition is obtained, for example, by heating a mixture containing adhesive components 4, 7 and the first conductive particles 5 and the second conductive particles 6 or dissolving the mixture in a solvent. As the solvent, for example, a solvent having a boiling point of 50 to 150° C. at normal pressure is used.

[0059] The adhesive film according to this embodiment can be used as an adhesive for bonding adherends of the same type to each other, and can also be used as an adhesive for bonding adherends of different types (for example, adherends having different thermal expansion coefficients) to each other. The adhesive film can be suitably used for connecting electronic components to each other.

[0060] Figure 2 FIG. 1 is a cross-sectional view schematically showing an example of the connection between electronic components. Figure 2As shown in (a), the adhesive film 1 involved in this embodiment is arranged between a first electronic component 10 and a second electronic component 13 to form a laminate 14. The first electronic component 10 includes a first substrate 8 and a first electrode 9 as a circuit electrode formed on the main surface of the first substrate 8, and the second electronic component 13 includes a second substrate 11 and a second electrode 12 formed on the main surface of the second substrate 11, for example, substantially the entire surface.

[0061] Next, the laminate 14 is heated while Figure 2 The second adhesive component 7 is pressed in the direction indicated by the arrow A in (a), so that the second adhesive component 7 flows to fill the recessed portion formed on the main surface of the first substrate 8. Figure 2 As shown in (b), the first electronic component 10 and the second electronic component 13 are electrically connected to each other via the circuit connecting material 15, thereby obtaining a connection structure 16. The heating temperature is, for example, 50 to 190° C. The pressure during pressurization is, for example, 0.1 to 30 MPa. These heating and pressurization are performed, for example, within the range of 0.5 to 120 seconds.

[0062] The first substrate 8 and the second substrate 11 may be substrates formed of glass, ceramic, polyimide, polycarbonate, polyester, polyethersulfone, etc. The first electrode 9 and the second electrode 12 may be electrodes formed of gold, silver, copper, tin, aluminum, ruthenium, rhodium, palladium, osmium, iridium, platinum, indium tin oxide (ITO), etc.

[0063] The circuit-connecting material 15 includes: the first conductive particles 5; the second conductive particles 6; and a cured product 17 of the adhesive components 4 and 7. That is, the circuit-connecting material 15 is obtained by curing the adhesive film 1 described above.

[0064] Even when the first electrode 9 is formed of a material (e.g., copper or aluminum) that easily forms an oxide film on its surface, the adhesive film 1 according to the present embodiment can suitably connect the electronic components 10 and 13 to each other. This is believed to be because the first conductive particles 5 and the second conductive particles 6 are used together in the adhesive film 1. Figure 2As shown in (b), the second conductive particles 6 form a main conductive path that connects the first electrode 9 and the second electrode 12 to each other, and on the other hand, the first conductive particles 5 assist the electrical connection between the second conductive particles 6 and the first electrode 9, thereby achieving a suitable connection. More specifically, the inventors speculate that since the first conductive particles 5 are dendrite-shaped conductive particles, even when an oxide film is formed on the surface of the first electrode 9, the first conductive particles 5 can penetrate the oxide film and contact the first electrode 9, and as a result, a suitable connection between the second conductive particles 6 and the first electrode 9 can be achieved. Therefore, it is believed that the adhesive film 1 involved in this embodiment has excellent reliability compared to an adhesive film using only one of the first conductive particles and the second conductive particles, that is, it can maintain the desired conductivity with respect to changes in ambient temperature.

[0065] Furthermore, the adhesive film 1 according to the present embodiment can further suitably connect the electronic components 10 and 13 to each other by having a first adhesive layer 2 and a second adhesive layer 3, wherein the first adhesive layer 2 contains a first adhesive component 4, a first conductive particle 5, and a second conductive particle 6, and the second adhesive layer 3 contains a second adhesive component 7. As the reason for this, it is considered that the second adhesive layer 3 has high fluidity because the volume ratio of the second adhesive component 7 in the second adhesive layer 3 is greater than the volume ratio of the first adhesive component 4 in the first adhesive layer 2. That is, it is considered that by using the second adhesive layer 3 with high fluidity, even for the first substrate 8 having unevenness on the main surface due to the first electrode 9, etc., the recess can be filled without gaps, and as a result, good bonding can be achieved. Therefore, it is considered that the adhesive film 1 according to the present embodiment has a further improved reliability compared with an adhesive film without a second adhesive layer.

[0066] Example

[0067] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to the following Examples.

[0068] (Preparation of Solution A1)

[0069] 50 g of a phenoxy resin (manufactured by Union Carbide Corporation, product name: PKHC, weight average molecular weight: 45,000) was dissolved in a mixed solvent of toluene (boiling point: 110.6° C.) and ethyl acetate (boiling point: 77.1° C.) (toluene:ethyl acetate = 1:1 in mass ratio) to obtain a phenoxy resin solution having a solid content of 40% by mass. In the phenoxy resin solution, urethane acrylate (manufactured by Negami Industry Co., Ltd., product name: UN7700) and phosphate dimethacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name: Light Ester P-2M) as free radical polymerizable substances, and 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane (manufactured by NOF Corporation, product name: Perhexa TMH) as a curing agent were mixed in a solid mass ratio of phenoxy resin:urethane acrylate:phosphate dimethacrylate:curing agent = 10:10:3:2 to obtain solution A1.

[0070] (Preparation of Solution A2)

[0071] 50 g of a phenoxy resin (manufactured by Union Carbide Corporation, product name: PKHC, weight average molecular weight: 45,000) was dissolved in a mixed solvent of toluene (boiling point: 110.6° C.) and ethyl acetate (boiling point: 77.1° C.) (toluene:ethyl acetate = 1:1 in mass ratio) to obtain a phenoxy resin solution having a solid content of 40% by mass. In the phenoxy resin solution, urethane acrylate (manufactured by Negami Industry Co., Ltd., product name: UN7700) and phosphate dimethacrylate (manufactured by Kyoeisha Chemical Co., Ltd., product name: Light Ester P-2M) as free radical polymerizable substances, and 1,1-bis(tert-hexylperoxy)-3,3,5-trimethylcyclohexane (manufactured by NOF Corporation, product name: Perhexa TMH) as a curing agent were mixed in a solid mass ratio of phenoxy resin:urethane acrylate:phosphate dimethacrylate:curing agent = 9:9:5:2 to obtain solution A2.

[0072] As the conductive particles B1 (first conductive particles), dendrite-shaped conductive particles (silver-coated copper particles, manufactured by Mitsui Mining and Co., Ltd., product name: ACBY-2) were used.

[0073] (Production of core body (resin particles))

[0074] Benzoyl peroxide as a polymerization initiator is added to a mixed solution of divinylbenzene, styrene monomer and butyl methacrylate, and the mixture is uniformly stirred at high speed while being heated to perform a polymerization reaction, thereby obtaining a particle dispersion. The particle dispersion is filtered and dried under reduced pressure to obtain a block as an agglomerate of particles. The block is further crushed to produce core bodies (resin particles) with an average particle diameter of 20 μm and different crosslinking densities.

[0075] (Production of Conductive Particles C1)

[0076] A palladium catalyst (made by Muromachi Technos Co., Ltd., product name: MK-2605) is carried on the surface of the above-mentioned core body, and a promoter (made by Muromachi Technos Co., Ltd., product name: MK-370) is used to activate the core body. The core body is put into a mixed solution of nickel sulfate aqueous solution, sodium hypophosphite aqueous solution and sodium tartrate aqueous solution heated to 60°C, and the pre-electrolytic plating process is carried out. The mixture is stirred for 20 minutes, and it is confirmed that the hydrogen bubbling stops. Next, a mixed solution of nickel sulfate, sodium hypophosphite, sodium citrate and a plating stabilizer is added, stirred until the pH is stable, and the post-electrolytic plating process is carried out until the hydrogen bubbling stops. Next, the plating solution is filtered, the filtrate is washed with water, and then dried in a vacuum dryer at 80°C to produce nickel-plated conductive particles C1 (second conductive particles).

[0077] [Example 1]

[0078] <Film formation of adhesive composition>

[0079] 45 parts by volume of conductive particles B1 and 15 parts by volume of conductive particles C1 were dispersed in 100 parts by volume of solution A1 to obtain a mixed solution. The obtained mixed solution was applied to a fluororesin film having a thickness of 80 μm, and the solvent was removed by hot air drying at 70°C for 10 minutes to obtain a film-like adhesive composition (first adhesive layer) having a thickness of 20 μm formed on the fluororesin film.

[0080] Next, 100 parts by volume of solution A2 was applied to a fluororesin film having a thickness of 80 μm, and the solvent was removed by hot air drying at 70°C for 10 minutes to obtain a film-like adhesive composition (second adhesive layer) having a thickness of 20 μm formed on the fluororesin film. The first adhesive layer was laminated on the second adhesive layer, and the fluororesin film was peeled off to obtain an adhesive film having a thickness of 40 μm.

[0081] The reliability of the obtained adhesive film when used as a circuit connecting material was evaluated by the reliability test shown below.

[0082] <Reliability test>

[0083] like Figure 3 As shown in (a) and (b), an adhesive film 21 cut into 6 mm × 6 mm is placed approximately in the center of a 6 mm × 50 mm copper foil 22, and attached by heating and pressing (50°C, 0.5 MPa, 2 seconds) using BD-07 manufactured by Ohashi Manufacturing Co., Ltd. Figure 3 As shown in (c), a component 25 (FPC manufactured by Hitachi Chemical Electronics Co., Ltd., size: 6 mm×50 mm, electrode spacing: 1000 μm, electrode: inter-electrode spacing = 11) having a copper electrode 24 with a thickness of 20 μm on a polyimide film 23 with a thickness of 25 μm was prepared. The component 25 was overlapped on the laminate of the copper foil 22 and the adhesive film 21 in a manner that the adhesive film 21 on the copper foil 22 was covered and the adhesive film 21 and the copper electrode 24 were in contact with each other. In this state, heating and pressing (150° C., 0.5 MPa, 10 seconds) were performed using BD-07 manufactured by Ohashi Manufacturing Co., Ltd., thereby obtaining a laminate as shown in FIG. Figure 4 (a) and (b) are mounting bodies for reliability testing. Figure 4 (b) along Figure 4 Sagittal cross-section along line IVb-IVb in (a).

[0084] like Figure 5 The obtained assembly was connected to an ammeter and a voltmeter, and the connection resistance (initial) was measured by a four-terminal method. In addition, a thermal cycle test was performed on the assembly using TSA-43EL manufactured by Espec Co., Ltd., in which the following thermal cycle was repeated 500 times, and then the connection resistance (after the thermal cycle test) was measured in the same manner as above. The results are shown in Table 1.

[0085] [Reference Example 1]

[0086] 45 parts by volume of conductive particles B1 and 15 parts by volume of conductive particles C1 were dispersed in 100 parts by volume of solution A1 to obtain a mixed solution. The obtained mixed solution was applied to a fluororesin film having a thickness of 80 μm, and the solvent was removed by hot air drying at 70°C for 10 minutes to obtain a film-like adhesive composition having a thickness of 30 μm formed on the fluororesin film. The obtained film-like adhesive composition was operated in the same manner as in Example 1 to evaluate its reliability when used as a circuit connection material. The results are shown in Table 1.

[0087] [Table 1]

[0088]

Claims

1. An adhesive film comprising a first adhesive layer and a second adhesive layer, The first adhesive layer contains: a first adhesive component; first conductive particles, which are dendrite-shaped conductive particles; and second conductive particles, which are conductive particles other than the first conductive particles and are conductive particles having a non-conductive core and a conductive layer disposed on the core. The second adhesive layer contains a second adhesive component. The volume ratio of the second adhesive component in the second adhesive layer is greater than the volume ratio of the first adhesive component in the first adhesive layer. 2 . The adhesive film according to claim 1 , wherein the second adhesive layer contains only the second adhesive component. 3 . The adhesive film according to claim 1 , wherein the conductive layer contains at least one selected from the group consisting of gold, nickel, and palladium.