Pre-lithiation binder, preparation method thereof, lithium ion battery diaphragm and lithium ion battery
A pre-lithiation binder with a biphenyl-lithium complex improves lithium-ion battery efficiency and cycle life by uniformly pre-lithiating the negative electrode, addressing safety and structural challenges.
Patent Information
- Application Number
- CN202411206099.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
Existing lithium-ion batteries suffer from low initial efficiency and poor cycle performance due to poor pre-lithiation effects, which can lead to safety hazards and structural instability.
A pre-lithiation binder with a biphenyl group in its polymer repeating unit, complexed with lithium ions, is applied between the lithium-ion battery separator and the negative electrode to achieve uniform pre-lithiation, improving the initial efficiency and cycle performance.
The pre-lithiation binder enhances the first-cycle coulombic efficiency and extends the cycle life of lithium-ion batteries by uniformly pre-lithiating the negative electrode, avoiding safety hazards and structural issues.
Smart Images

Figure CN119081592A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion batteries, and in particular to a pre-lithiation binder, a preparation method thereof, a lithium ion battery separator and a lithium ion battery. Background Art
[0002] During the first charge and discharge process of lithium-ion batteries, the formation of SEI film on the negative electrode consumes active lithium, resulting in irreversible capacity loss. At the same time, emerging high-capacity negative electrode materials, such as silicon-based materials, have large volume changes during the lithium extraction process and poor cycle performance. Therefore, researchers choose to use pre-lithiation technology to directly add additional active lithium to the negative electrode, or first add additional active lithium to the positive electrode and then release the active lithium to the negative electrode during the first charge process to compensate for the poor cyclability. In other words, pre-lithiation technology can achieve: (1) compensate for the loss of active lithium and improve the battery's first coulombic efficiency and energy density; (2) cause the negative electrode to expand in volume in advance to avoid structural collapse due to large volume changes in the negative electrode during subsequent cyclic charge and discharge processes, thereby increasing the battery's cycle life.
[0003] However, the use of lithium metal to directly pre-lithiate the negative electrode, such as lithium foil, or the use of stabilized lithium metal powder to contact the negative electrode to react chemically to achieve pre-lithiation, the corresponding pre-lithiation rate and degree cannot be controlled, and it is easy to over-pre-lithiate, resulting in lithium precipitation on the negative electrode, causing safety hazards. In addition, lithium metal, as an additional electrode introduced, is electrochemically pre-lithiated with the negative electrode to form a temporary battery, which is incompatible with the current lithium-ion battery production process. Moreover, the chemical properties of lithium metal are active and it is easy to react and deteriorate with air and moisture, making the industrialization of lithium metal pre-lithiation difficult. For positive electrode pre-lithiation, such as adding lithium-rich additives to the positive electrode sheet, the additive will form poorly conductive residues or defects in the positive electrode sheet after decomposition, increase the charge transfer resistance of the positive electrode sheet or destroy the structure of the positive electrode sheet, and over-lithiation of the positive electrode active material is likely to cause its structure to be unstable or even destroyed.
[0004] Based on this, how to provide a pre-lithiation binder and apply it between the lithium-ion battery separator and the lithium-ion battery negative electrode plate, so as to effectively realize the pre-lithiation of the lithium-ion battery negative electrode plate and improve the initial efficiency and cycle performance of the final lithium-ion battery, is one of the technical problems that need to be solved in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide a pre-lithiation binder, a preparation method thereof, a lithium ion battery separator and a lithium ion battery, so as to solve the problem that the pre-lithiation effect of lithium ion battery pole pieces in the prior art is poor, resulting in low initial efficiency and poor cycle performance of the obtained lithium ion battery.
[0006] In order to achieve the above object, the first aspect of the present invention provides a pre-lithiation binder having a structure shown in Formula I:
[0007]
[0008] Wherein, R1 and R2 are independently selected from vacancy, halogen, substituted or unsubstituted C1-C5 alkyl and C2-C6 alkyl ester, and R1 and R2 are both connected to the benzene ring in the form of a single bond, n1 is any integer from 0 to 4, n2 is any integer from 0 to 5, and n is 4500 to 5000.
[0009] The pre-lithiation binder provided by the present invention has a biphenyl group in its polymer repeating unit in a reduced state and complexed with lithium ions; when the special lithium-biphenyl complex group thereon is in direct contact with the negative electrode active material of the lithium ion battery, the biphenyl group can reduce the negative electrode active material, and the complexed lithium ions thereon are simultaneously embedded in the negative electrode, thereby achieving uniform pre-lithiation of the negative electrode sheet, thereby improving the initial efficiency and cycle performance of the final lithium ion battery.
[0010] Furthermore, the lithiated binder has a structure shown in Formula I-1 or Formula I-2:
[0011]
[0012] Wherein, R1 is empty, R2 is selected from empty, halogen, substituted or unsubstituted C1-C3 alkyl and C2-C4 ester, and n2 is any integer from 1 to 3.
[0013] The inventors designed the molecular structure of the pre-lithiation binder polymer through a large number of experiments and found that when the ester group is located at the ortho or meta position of the biphenyl, the above structure has a better lithium supplementation effect.
[0014] Furthermore, the lithiated binder has a structure shown in Formula I-3:
[0015]
[0016] Among them, R1 is selected from vacant, halogen and substituted or unsubstituted C1-C3 alkyl, and n1 is any integer from 0 to 2; R2 is selected from vacant, halogen, substituted or unsubstituted C1-C3 alkyl and C2-C4 ester, and n2 is any integer from 1 to 3.
[0017] When the ester group is located at the para position of the biphenyl, the inventors also designed and optimized the substituents thereon through a large number of experiments, and found that when it is the above situation, the obtained pre-lithiation binder has a better lithium replenishing effect.
[0018] Further, R1 and R2 are each independently selected from H, F, Cl, methyl or methyl ester, and n1 and n2 are each independently 0, 1 or 2. In this case, the lithium supplementation effect of the pre-lithiation binder polymer side chain is more significantly optimized.
[0019] Further, the pre-lithiation binder is selected from one or more of the following structures:
[0020]
[0021]
[0022] Further, the pre-lithiation binder is selected from any two of the following structures:
[0023]
[0024] After a large number of experiments, the inventors have optimized the structures of the above-mentioned specific pre-lithiation binder polymers, and found that when it is one or more of the above structures, the lithium replenishment effect of the obtained pre-lithiation binder is better, that is, it can more effectively optimize the initial efficiency and cycle of the final lithium-ion battery.
[0025] Preferably, the pre-lithiation binder is:
[0026] And x+y=n, x:y=0.8~1.2.
[0027] The second aspect of the present invention provides a method for preparing the above-mentioned pre-lithiation binder, comprising: step S1, preparing polybiphenyl acrylate; step S2, preparing a lithium-containing organic solution; step S3, adding polybiphenyl acrylate to the lithium-containing organic solution for reaction to obtain a pre-lithiation binder; the structure of polybiphenyl acrylate is:
[0028]
[0029] Furthermore, the molar ratio of lithium to polybiphenyl acrylate is (1.1-1.5):1; preferably, the reaction time is 1-3 hours, and the reaction is carried out under the protection of nitrogen and / or argon.
[0030] In order to enhance the complexing effect between lithium ions and biphenyl groups in polybiphenyl acrylate and to prevent the structure of the obtained pre-lithiation binder from being destroyed, thereby enhancing the bonding force of the obtained pre-lithiation binder, the above experimental conditions are preferably selected.
[0031] Furthermore, the reaction temperature is 25±2°C, and the solvent used to prepare the organic solution is tetrahydrofuran. Under these conditions, a pre-lithiation binder is obtained that has more significant improvements in the first efficiency and cycle of lithium-ion batteries.
[0032] A third aspect of the present invention provides a lithium ion separator, comprising a base film and a coating disposed on one surface of the base film, wherein the coating comprises the above-mentioned pre-lithiation binder.
[0033] The diaphragm with a coating formed by a pre-lithiation binder provided by the present invention can be tightly combined with a lithium-ion negative electrode sheet while preventing short circuits, and can replenish lithium for the negative electrode active material, thereby effectively improving the initial efficiency and cycle of the resulting lithium-ion battery.
[0034] Furthermore, based on the total weight of the coating being 100%, the weight of the pre-lithiation binder accounts for 10% to 40%; preferably, the thickness of the coating is 1 μm to 3 μm, and the number of coating layers is 1 or 2.
[0035] The above-mentioned setting is more conducive to coordinating the adhesion, insulation, ion transfer ability, mechanical properties and pre-lithiation function of the coating, thereby obtaining a lithium-ion battery with better electrical performance.
[0036] The fourth aspect of the present invention provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, the negative electrode sheet comprising a negative electrode collector and a negative electrode active layer arranged on at least one side surface of the negative electrode collector, the positive electrode sheet comprising a positive electrode collector and a positive electrode active layer arranged on at least one side surface of the positive electrode collector, the separator is arranged between the negative electrode active layer of the negative electrode sheet and the positive electrode active layer of the positive electrode sheet, the separator is the above-mentioned lithium-ion battery separator, and the coating of the lithium-ion battery separator is arranged in contact with the negative electrode active layer.
[0037] The obtained lithium-ion battery exhibits higher first-cycle coulombic efficiency and long-cycle stability because its structure contains a separator that can uniformly provide lithium ions.
[0038] By applying the technical solution of the present invention, a pre-lithiation binder of polybiphenyl acrylate polymer is provided. After the lithium-ion battery is injected, the biphenyl group in the structure of the pre-lithiation binder can reduce the negative electrode active material, and the lithium ions complexed thereon are simultaneously embedded in the negative electrode to achieve pre-lithiation of the negative electrode. The pre-lithiation binder provided by the present invention is uniformly pre-lithiated, is compatible with the current lithium-ion battery production process, and can significantly improve the first efficiency and cycle life of the lithium-ion battery. DETAILED DESCRIPTION
[0039] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0040] As described in the background art, the prior art has the problem that lithium-ion batteries have low initial efficiency and poor cycle performance due to poor pre-lithiation effect of the pole piece. In order to solve the above technical problems, the first aspect of the present invention provides a pre-lithiation binder having a structure shown in Formula I:
[0041]
[0042] Wherein, each repeating unit includes a biphenyl free radical and a lithium ion complexed with the biphenyl free radical; R1 and R2 are each independently selected from a null, a halogen, a substituted or unsubstituted C1-C5 alkyl group and a C2-C6 alkyl ester group, and R1 and R2 are both connected to the benzene ring in a single bond manner, n1 is any integer from 0 to 4, n2 is any integer from 0 to 5, and n is 4500 to 5000.
[0043] The pre-lithiation binder provided by the present invention has a biphenyl group in its polymer repeating unit in a reduced state and complexed with lithium ions; when the special lithium-biphenyl complex group thereon is in direct contact with the negative electrode active material of the lithium ion battery, the biphenyl group can reduce the negative electrode active material, and the complexed lithium ions thereon are simultaneously embedded in the negative electrode, thereby achieving uniform pre-lithiation of the negative electrode sheet, thereby improving the initial efficiency and cycle performance of the final lithium ion battery.
[0044] In particular, compared to the lithium-biphenyl pre-lithiation reagent used in the art, that is, an organic solvent system containing biphenyl radical anions and lithium ion complexes, the binder containing biphenyl radical anions and lithium ion complex groups provided by the present invention is used for the diaphragm coating, which can realize the in-situ pre-lithiation of the negative electrode active material after the lithium ion battery is assembled and injected, avoiding the non-in-situ pre-lithiation of the negative electrode active material before the battery is assembled, resulting in a higher reaction activity of the negative electrode active material after pre-lithiation, and side reactions are prone to occur when encountering air and moisture during the subsequent assembly process.
[0045] In several preferred embodiments, the lithiated binder has a structure shown in Formula I-1 or Formula I-2:
[0046]
[0047] Wherein, R1 is empty, R2 is selected from empty, halogen, substituted or unsubstituted C1-C3 alkyl and C2-C4 ester, and n2 is any integer from 1 to 3. The inventors designed the molecular structure of the pre-lithiation binder polymer through a large number of experiments, and found that when the ester group is located at the ortho or meta position of the biphenyl, the above structure has a better lithium supplementation effect.
[0048] In several more preferred embodiments, the inventors further prefer structures with better lithium supplementation effects, wherein R2 is selected from one or more of vacancy, methyl, ethyl, methyl formate and ethyl formate.
[0049] In several preferred embodiments, the lithiated binder has a structure shown in Formula I-3:
[0050]
[0051] Wherein, R1 is selected from vacancy, halogen, and substituted or unsubstituted C1-C3 alkyl, and n1 is any integer from 0 to 2; R2 is selected from vacancy, halogen, substituted or unsubstituted C1-C3 alkyl, and C2-C4 ester, and n2 is any integer from 1 to 3. When the ester group is located at the para position of the biphenyl, the inventors also designed and optimized the substituents thereon through a large number of experiments, and found that when it is the above situation, the obtained pre-lithiation binder has a better lithium supplementation effect.
[0052] In several more preferred embodiments, R1 is void, fluorine or chlorine; R2 is selected from one or more of void, chlorine, fluorine, methyl, ethyl, methyl formate and ethyl formate. In this case, the obtained structure is more stable and has a higher lithium replenishment effect.
[0053] In order to further optimize the lithium replenishment effect of the pre-lithiation binder polymer side chain, the inventors preferably select R1 and R2 from H, F, Cl, methyl or methyl ester groups independently, and n1 and n2 are 0, 1 or 2 independently after a large number of experiments.
[0054] In several preferred embodiments, the pre-lithiation binder is selected from one or more of the following structures:
[0055]
[0056] After a large number of experiments, the inventors have optimized the above-mentioned specific pre-lithiation binder polymer structures, and found that when its structure is one or more of the above structures, the obtained pre-lithiation binder has a better lithium replenishment effect, that is, it can more effectively optimize the initial efficiency and cycle of the final lithium-ion battery.
[0057] In order to improve the lithium supplementation effect, the inventors further preferred the pre-lithiation binder to be selected from any two of the following structures after a large number of experiments:
[0058]
[0059] And, more preferably the pre-lithiation binder is:
[0060] And x+y=n, x:y=0.8~1.2.
[0061] The second aspect of the present invention provides a method for preparing the above-mentioned pre-lithiation binder, comprising: step S1, preparing polybiphenyl acrylate; step S2, preparing a lithium-containing organic solution; step S3, adding polybiphenyl acrylate to the lithium-containing organic solution for reaction to obtain a pre-lithiation binder; the structure of polybiphenyl acrylate is:
[0062]
[0063] R1, R2, n1, n2, and n in the above polybiphenyl acrylate have the same definitions as described above.
[0064] Specifically, in the lithium-containing organic solution, lithium exists in the form of lithium metal element.
[0065] The present invention provides a preparation method for the above-mentioned pre-lithiation binder. The process of preparing polybiphenyl acrylate further includes:
[0066] Step S1-1, dissolving acryloyl chloride in tetrahydrofuran to obtain a first reaction solution; dissolving triethylamine and hydroxybiphenyl in tetrahydrofuran to obtain a second reaction solution; adding the first reaction solution dropwise to the second reaction solution, the reaction temperature is 0°C, and the reaction time is 1 to 3 hours; after the reaction is completed, filtering to obtain biphenyl acrylate;
[0067] Among them, the structure of acryloyl chloride is The structure of hydroxybiphenyl is The structure of the biphenyl acrylate obtained by the reaction of the two is correspondingly
[0068] (One or more biphenyl acrylates are selected according to the structure of the pre-lithiation binder to be formed, and the amount thereof is set according to the ratio of x to y).
[0069] Step S1-2, dissolving the above-mentioned biphenyl acrylate and azobisisobutyronitrile obtained in S1-1 into toluene to obtain a third reaction liquid; placing the third reaction liquid in a nitrogen or argon atmosphere, the reaction temperature is 60-80°C, and the reaction time is 6-8h; pouring the third reaction liquid after the reaction into methanol for precipitation, and filtering to obtain the above-mentioned polybiphenyl acrylate.
[0070] Of course, in addition to the above-mentioned synthetic route provided by the present invention, the synthetic route commonly used in the art can also be used to prepare polybiphenyl acrylate.
[0071] In several typical embodiments, in order to enhance the complexing effect between lithium ions and biphenyl groups in polybiphenyl acrylate, and to prevent the structure of the obtained pre-lithiation binder from being destroyed, thereby enhancing the bonding strength of the obtained pre-lithiation binder, the inventors have optimized the reaction molar ratio of lithium to polybiphenyl acrylate to (1.1-1.5):1 through a large number of experiments, the reaction time is 1-3h, and the reaction is carried out under nitrogen and / or argon protection. The reaction temperature is 25±2°C, and the solvent used to prepare the organic solution is tetrahydrofuran. Under these conditions, a pre-lithiation binder with more significant improvements in the first effect and cycle of lithium-ion batteries is obtained.
[0072] The third aspect of the present invention provides a lithium ion separator, comprising a base film and a coating disposed on one side of the base film, wherein the coating comprises the above-mentioned pre-lithiation binder. The separator provided by the present invention with a coating formed by the pre-lithiation binder can be tightly combined with the lithium ion negative electrode sheet while preventing short circuit, and replenish lithium for the negative electrode active material, thereby effectively improving the initial efficiency and cycle of the obtained lithium ion battery.
[0073] In several preferred embodiments, in order to coordinate the adhesion, insulation, ion transfer ability and pre-lithiation function of the coating, the inventors have preferably determined through a large number of experiments that the weight of the pre-lithiation binder is 10% to 40% based on the total weight of the coating as 100%, thereby obtaining a lithium-ion battery with better electrical performance. Also, in order to improve the mechanical properties of the diaphragm, the thickness of the coating is preferably 1 μm to 3 μm, and the number of coatings is 1 or 2 layers, thereby more effectively improving the long-cycle stability of the lithium-ion battery.
[0074] Furthermore, the coating on the base film is a first coating and a second coating stacked in sequence in a direction away from the base film, and both the first coating and the second coating contain a pre-lithiation binder. The first coating is an inorganic non-metallic coating containing aluminum oxide, and the second coating is an organic coating containing a polyvinylidene fluoride binder. The setting of the two layers of coating, in addition to being able to achieve a uniform pre-lithiation effect, is more conducive to adjusting the amount of the pre-lithiation binder.
[0075] The fourth aspect of the present invention provides a lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the negative electrode sheet comprises a negative current collector and a negative electrode active layer disposed on at least one side of the surface of the negative current collector, the positive electrode sheet comprises a positive current collector and a positive electrode active layer disposed on at least one side of the surface of the positive current collector, the separator is disposed between the negative electrode active layer of the negative electrode sheet and the positive electrode active layer of the positive electrode sheet, the separator is the above-mentioned lithium ion battery separator, and the coating of the lithium ion battery separator is disposed in contact with the negative electrode active layer. The obtained lithium ion battery exhibits higher first cycle coulomb efficiency and long cycle stability because its structure includes a separator that can uniformly provide lithium ions.
[0076] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0077] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0078] Example 1
[0079] 1. Preparation of pre-lithiation binder: dissolve acryloyl chloride (CAS No.: 814-68-6) in tetrahydrofuran to obtain a first reaction solution; dissolve triethylamine (CAS No.: 121-44-8) and 2'-methyl-2-hydroxybiphenyl (CAS No.: 77897-02-0) in tetrahydrofuran to obtain a second reaction solution; add the first reaction solution dropwise to the second reaction solution, the molar ratio of acryloyl chloride, triethylamine and 2'-methyl-2-hydroxybiphenyl is 1.2:1.2:1, the reaction temperature is 0°C, and the reaction time is 1h; after the reaction is completed, filter to obtain biphenyl acrylate. Dissolve biphenyl acrylate and azobisisobutyronitrile (CAS No.: 78-67-1) in toluene to obtain a third reaction solution, wherein the molar ratio of biphenyl acrylate to azobisisobutyronitrile is 300:1; place the third reaction solution in a nitrogen atmosphere, the reaction temperature is 80°C, and the reaction time is 6 hours; pour the third reaction solution after the reaction into methanol for precipitation, and filter to obtain polybiphenyl acrylate. In a nitrogen atmosphere, dissolve lithium metal in tetrahydrofuran to obtain a fourth reaction solution; add polybiphenyl acrylate to the fourth reaction solution, wherein the molar ratio of lithium metal to polybiphenyl acrylate is 1.1:1, the reaction temperature is room temperature (25°C), and the reaction time is 1 hour; after the reaction, filter and wash with methanol to obtain a pre-lithiation binder, wherein n is 4600-4900. The reaction formula is as follows.
[0080]
[0081] 2. Preparation of pre-lithiation membrane: Alumina, the above-mentioned pre-lithiation binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecyne diol polyether wetting agent, and water are uniformly mixed in a mass percentage of 23.2:16:0.2:0.5:0.1:60 to obtain a slurry, which is coated on a 9μm polyethylene base film with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 40wt%, to obtain a pre-lithiation membrane.
[0082] Example 2
[0083] 1. Preparation of pre-lithiation binder: dissolve acryloyl chloride in tetrahydrofuran to obtain a first reaction solution; dissolve triethylamine and 4'-methyl formate-3-hydroxybiphenyl (CAS No.: 579511-01-6) in tetrahydrofuran to obtain a second reaction solution; add the first reaction solution dropwise to the second reaction solution, the molar ratio of acryloyl chloride, triethylamine, and 4'-methyl formate-3-hydroxybiphenyl is 1.3:1.2:1, the reaction temperature is 0°C, and the reaction time is 2h; after the reaction is completed, filter to obtain biphenyl acrylate. Dissolve biphenyl acrylate and azobisisobutyronitrile in toluene to obtain a third reaction solution, the molar ratio of biphenyl acrylate and azobisisobutyronitrile is 310:1; place the third reaction solution in a nitrogen atmosphere, the reaction temperature is 60°C, and the reaction time is 8h; after the reaction is completed, pour the third reaction solution into methanol for precipitation, and filter to obtain polybiphenyl acrylate. In a nitrogen atmosphere, lithium metal is dissolved in tetrahydrofuran to obtain a fourth reaction solution; polybiphenyl acrylate is added to the fourth reaction solution, the molar ratio of lithium metal to polybiphenyl acrylate is 1.3:1, the reaction temperature is room temperature, and the reaction time is 2 hours; after the reaction is completed, the pre-lithiation binder is obtained by filtering and washing with methanol, wherein n is 4600-4900. The reaction formula is as follows.
[0084]
[0085] 2. Preparation of pre-lithiation membrane: Alumina, the above-mentioned pre-lithiation binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecynediol polyether wetting agent, and water are uniformly mixed in a mass percentage of 27.2:12:0.2:0.5:0.1:60 to obtain a slurry, which is applied on a 9μm polyethylene base film with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 30wt%; polyvinylidene fluoride binder, the above-mentioned pre-lithiation binder, sodium dodecylbenzene sulfonate dispersant, and water are uniformly mixed in a mass percentage of 13.9:6:0.1:80 to obtain a slurry, which is applied on the above-mentioned membrane with a coating thickness of 1μm and dried. The content of the pre-lithiation binder in the coating is 30wt%, thereby obtaining a pre-lithiation membrane.
[0086] Example 3
[0087] 1. Preparation of pre-lithiation binder: dissolve acryloyl chloride in tetrahydrofuran to obtain a first reaction solution; dissolve triethylamine and 4'-chloro-4-hydroxybiphenyl (CAS No.: 28034-99-3) in tetrahydrofuran to obtain a second reaction solution; add the first reaction solution dropwise to the second reaction solution, the molar ratio of acryloyl chloride, triethylamine, and 4'-chloro-4-hydroxybiphenyl is 1.4:1.3:1, the reaction temperature is 0°C, and the reaction time is 2.5h; after the reaction is completed, filter to obtain biphenyl acrylate. Dissolve biphenyl acrylate and azobisisobutyronitrile in toluene to obtain a third reaction solution, the molar ratio of biphenyl acrylate and azobisisobutyronitrile is 320:1; place the third reaction solution in a nitrogen atmosphere, the reaction temperature is 70°C, and the reaction time is 7h; after the reaction is completed, pour the third reaction solution into methanol for precipitation, and filter to obtain polybiphenyl acrylate. In a nitrogen atmosphere, lithium metal is dissolved in tetrahydrofuran to obtain a fourth reaction solution; polybiphenyl acrylate is added to the fourth reaction solution, the molar ratio of lithium metal to polybiphenyl acrylate is 1.4:1, the reaction temperature is room temperature, and the reaction time is 2 hours; after the reaction is completed, the pre-lithiation binder is obtained by filtering and washing with methanol, wherein n is 4600-4800. The reaction formula is as follows.
[0088]
[0089] 2. Preparation of pre-lithiation membrane: Alumina, the above-mentioned pre-lithiation binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecynediol polyether wetting agent, and water are uniformly mixed in a mass percentage of 31.2:8:0.2:0.5:0.1:60 to obtain a slurry, which is applied on a 9μm polyethylene base film with a coating thickness of 2μm and dried. The content of the pre-lithiation binder in the coating is 20wt%; polyvinylidene fluoride binder, the above-mentioned pre-lithiation binder, sodium dodecylbenzene sulfonate dispersant, and water are uniformly mixed in a mass percentage of 14.9:10:0.1:75 to obtain a slurry, which is applied on the above-mentioned membrane with a coating thickness of 2μm and dried. The content of the pre-lithiation binder in the coating is 40wt%, thereby obtaining a pre-lithiation membrane.
[0090] Example 4
[0091] 1. Preparation of pre-lithiation binder: dissolve acryloyl chloride in tetrahydrofuran to obtain a first reaction solution; dissolve triethylamine and 3'-methyl formate-4'-fluoro-4-hydroxybiphenyl (CAS No.: 1261900-28-0) in tetrahydrofuran to obtain a second reaction solution; add the first reaction solution dropwise to the second reaction solution, the molar ratio of acryloyl chloride, triethylamine, and 3'-methyl formate-4'-fluoro-4-hydroxybiphenyl is 1.3:1.2:1, the reaction temperature is 0°C, and the reaction time is 1.5h; after the reaction is completed, filter to obtain biphenyl acrylate. Dissolve biphenyl acrylate and azobisisobutyronitrile in toluene to obtain a third reaction solution, the molar ratio of biphenyl acrylate and azobisisobutyronitrile is 330:1; place the third reaction solution in a nitrogen atmosphere, the reaction temperature is 60°C, and the reaction time is 8h; pour the third reaction solution after the reaction into methanol for precipitation, and filter to obtain polybiphenyl acrylate. In a nitrogen atmosphere, lithium metal is dissolved in tetrahydrofuran to obtain a fourth reaction solution; polybiphenyl acrylate is added to the fourth reaction solution, the molar ratio of lithium metal to polybiphenyl acrylate is 1.5:1, the reaction temperature is room temperature, and the reaction time is 3 hours; after the reaction is completed, the pre-lithiation binder is obtained by filtering and washing with methanol, wherein n is 4500-4700. The reaction formula is as follows.
[0092]
[0093] 2. Preparation of pre-lithiation membrane: Alumina, the above-mentioned pre-lithiation binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecynediol polyether wetting agent, and water are uniformly mixed in a mass percentage of 26.2:3:0.2:0.5:0.1:70 to obtain a slurry, which is applied on a 9μm polyethylene base film with a coating thickness of 1μm and dried. The content of the pre-lithiation binder in the coating is 10wt%; polyvinylidene fluoride binder, the above-mentioned pre-lithiation binder, sodium dodecylbenzene sulfonate dispersant, and water are uniformly mixed in a mass percentage of 15.9:9:0.1:75 to obtain a slurry, which is applied on the above-mentioned membrane with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 36wt%, thereby obtaining a pre-lithiation membrane.
[0094] Example 5
[0095] 1. Preparation of pre-lithiation binder: dissolve acryloyl chloride in tetrahydrofuran to obtain a first reaction solution; dissolve triethylamine, 4-hydroxybiphenyl (CAS No.: 92-69-3) and 2-fluoro-4-hydroxybiphenyl (CAS No.: 477860-13-2) in tetrahydrofuran to obtain a second reaction solution; add the first reaction solution dropwise to the second reaction solution, the molar ratio of acryloyl chloride, triethylamine, 4-hydroxybiphenyl and 2-fluoro-4-hydroxybiphenyl is 1.2:1.2:0.5:0.5, the reaction temperature is 0°C, and the reaction time is 1h; after the reaction is completed, filter to obtain biphenyl acrylate. Dissolve biphenyl acrylate and azobisisobutyronitrile in toluene to obtain a third reaction solution, wherein the molar ratio of biphenyl acrylate to azobisisobutyronitrile is 340:1; place the third reaction solution in a nitrogen atmosphere, the reaction temperature is 60°C, and the reaction time is 8 hours; pour the third reaction solution after the reaction into methanol for precipitation, and filter to obtain polybiphenyl acrylate. In a nitrogen atmosphere, dissolve lithium metal in tetrahydrofuran to obtain a fourth reaction solution; add polybiphenyl acrylate to the fourth reaction solution, wherein the molar ratio of lithium metal to polybiphenyl acrylate is 1.3:1, the reaction temperature is room temperature, and the reaction time is 2 hours; after the reaction, filter and wash with methanol to obtain a pre-lithiation binder, wherein x:y is 1, and x+y is 4500-5000.
[0096] The reaction formula is as follows.
[0097]
[0098] 2. Preparation of pre-lithiation membrane: Alumina, the above-mentioned pre-lithiation binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecynediol polyether wetting agent, and water are uniformly mixed in a mass percentage of 27.2:12:0.2:0.5:0.1:60 to obtain a slurry, which is applied on a 9μm polyethylene base film with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 30wt%; polyvinylidene fluoride binder, the above-mentioned pre-lithiation binder, sodium dodecylbenzene sulfonate dispersant, and water are uniformly mixed in a mass percentage of 22.4:2.5:0.1:75 to obtain a slurry, which is applied on the above-mentioned membrane with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 10wt%, thereby obtaining a pre-lithiation membrane.
[0099] Example 6
[0100] 1. Preparation of pre-lithiation binder: dissolve acryloyl chloride in tetrahydrofuran to obtain a first reaction solution; dissolve triethylamine, 3-hydroxybiphenyl (CAS No.: 580-51-8) and 4'-methyl-4-hydroxybiphenyl (CAS No.: 26191-64-0) in tetrahydrofuran to obtain a second reaction solution; add the first reaction solution dropwise to the second reaction solution, the molar ratio of acryloyl chloride, triethylamine, 3-hydroxybiphenyl and 4'-methyl-4-hydroxybiphenyl is 1.5:1.3:0.5:0.5, the reaction temperature is 0°C, and the reaction time is 3h; after the reaction is completed, filter to obtain biphenyl acrylate. Dissolve biphenyl acrylate and azobisisobutyronitrile in toluene to obtain a third reaction solution, wherein the molar ratio of biphenyl acrylate to azobisisobutyronitrile is 350:1; place the third reaction solution in a nitrogen atmosphere, the reaction temperature is 60°C, and the reaction time is 8 hours; pour the third reaction solution after the reaction into methanol for precipitation, and filter to obtain polybiphenyl acrylate. In a nitrogen atmosphere, dissolve lithium metal in tetrahydrofuran to obtain a fourth reaction solution; add polybiphenyl acrylate to the fourth reaction solution, wherein the molar ratio of lithium metal to polybiphenyl acrylate is 1.2:1, the reaction temperature is room temperature, and the reaction time is 1.5 hours; after the reaction, filter and wash with methanol to obtain a pre-lithiation binder, wherein x:y is 1, x+y is 4700-5000, and the reaction formula is as follows.
[0101]
[0102] 2. Preparation of pre-lithiation membrane: Alumina, the above-mentioned pre-lithiation binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecynediol polyether wetting agent, and water are uniformly mixed in mass percentages of 23.2:16:0.2:0.5:0.1:60 to obtain a slurry, which is applied on a 9μm polyethylene base film with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 40wt%; polyvinylidene fluoride binder, the above-mentioned pre-lithiation binder, sodium dodecylbenzene sulfonate dispersant, and water are uniformly mixed in mass percentages of 14.9, 10, 0.1, and 75 to obtain a slurry, which is applied on the above-mentioned membrane with a coating thickness of 3μm and dried. The content of the pre-lithiation binder in the coating is 40wt%, thereby obtaining a pre-lithiation membrane.
[0103] Example 7
[0104] The only difference between this embodiment and embodiment 1 is that the molar ratio of lithium metal to polybiphenyl acrylate in the fourth reaction solution is 0.5:1, and the reaction time is 0.5 h.
[0105] Example 8
[0106] The only difference between this embodiment and embodiment 1 is that the molar ratio of lithium metal to polybiphenyl acrylate in the fourth reaction solution is 2:1, and the reaction time is 3.5 hours.
[0107] Application Comparative Example 1
[0108] Alumina, polyacrylic acid binder, sodium polyacrylate dispersant, sodium carboxymethyl cellulose thickener, dodecyne glycol polyether wetting agent and water are uniformly mixed in a mass percentage of 23.2:16:0.2:0.5:0.1:60 to obtain a slurry, which is coated on a 9 μm polyethylene base film with a coating thickness of 3 μm and dried. The content of polyacrylic acid binder in the coating is 40wt%, to obtain a lithium ion battery separator.
[0109] That is, the difference between this comparative application example and Example 1 is that a polyacrylic acid binder without a pre-lithiation function is used in the diaphragm coating, and its content is the same as that in Example 1.
[0110] Test Method
[0111] Battery assembly: The coating of the pre-lithiation separator obtained in each embodiment is placed opposite to the graphite negative electrode sheet, and a lithium iron phosphate positive electrode sheet is used, and the pre-lithiation soft-pack battery is obtained through lamination, aluminum-plastic film packaging, liquid injection and infiltration.
[0112] Battery performance test: The soft-pack battery samples obtained above were formed and divided at 45°C and 25°C respectively, and the first coulombic efficiency of the battery was calculated. The soft-pack battery samples obtained above were subjected to 800 cycles of cycle performance test at 25°C and 1C rate, and their capacity retention rate was calculated. The results are shown in Table 1.
[0113] Table 1
[0114] First coulombic efficiency (%) Capacity retention after 800 cycles (%) Example 1 94.6 100.9 Example 2 94.3 101.3 Example 3 94.4 101.2 Example 4 94.2 100.8 Example 5 94.3 100.6 Example 6 96.5 102.4 Example 7 91.3 97.4 Example 8 94.5 96.0 Application Comparative Example 1 90.6 95.2
[0115] From the above description, it can be seen that the pre-lithiation binder provided by the present invention, after being used as one of the components to form a lithium-ion battery separator, the resulting separator can uniformly pre-lithiate the negative electrode of the lithium-ion battery, thereby effectively improving the initial efficiency and cycle of the lithium-ion battery.
[0116] Specifically, compared with the comparative example in which the diaphragm coating uses a polyacrylic acid binder without pre-lithiation function, the diaphragm coatings of Examples 1-5 use the same mass proportion of pre-lithiation binder, and the first coulombic efficiency of the corresponding lithium-ion battery can be increased by 4%, the capacity retention rate after 800 cycles can be increased by 6%, and the capacity retention rate is greater than 100%, and there is no capacity decay; Example 6 increases the mass proportion of the pre-lithiation binder in the diaphragm coating, and the first coulombic efficiency of the corresponding lithium-ion battery can be increased by 6%, the capacity retention rate after 800 cycles can be increased by 7%, and the capacity retention rate is greater than 100%, and there is no capacity decay. It is worth noting that in the process of preparing the pre-lithiation binder, the reaction molar ratio of the lithium metal organic solution to polybiphenyl acrylate is less than 1.1, and the reaction time is less than 1h. The biphenyl groups are not fully reduced and the lithium ions are not fully complexed, which reduces the pre-lithiation effect, that is, the first coulombic efficiency and capacity retention rate of the corresponding lithium-ion battery are not improved enough; or the reaction molar ratio of the lithium metal organic solution to polybiphenyl acrylate is greater than 1.5, and the reaction time is greater than 3h. The structure of the obtained pre-lithiation binder is destroyed, the bonding force is insufficient, and the cycle performance of the corresponding lithium-ion battery is affected.
[0117] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A pre-lithiation binder, It is characterized in that The pre-lithiation binder has a structure shown in Formula I: R 1 and R 2 are independently selected from null, halogen, substituted or unsubstituted C1-C5 alkyl and C2-C6 alkyl ester groups, and R 1 and R 2 They are all connected to the benzene ring in the form of a single bond, n1 is any integer from 0 to 4, n2 is any integer from 0 to 5, and n is 4500 to 5000.
2. The pre-lithiation binder according to claim 1, It is characterized in that The pre-lithiation binder has a structure shown in Formula I-1 or Formula I-2: Among them, R 1 Empty, R 2 It is selected from the group consisting of vacancy, halogen, substituted or unsubstituted C1-C3 alkyl and C2-C4 ester, and n2 is any integer from 1 to 3.
3. The pre-lithiation binder according to claim 1, It is characterized in that The pre-lithiation binder has a structure shown in Formula I-3: Among them, R 1 is selected from the group consisting of vacancy, halogen, and substituted or unsubstituted C1-C3 alkyl, n1 is any integer from 0 to 2; R 2 It is selected from the group consisting of vacancy, halogen, substituted or unsubstituted C1-C3 alkyl and C2-C4 ester, and n2 is any integer from 1 to 3.
4. The pre-lithiation binder according to any one of claims 1 to 3, It is characterized in that R 1 and R 2 Each is independently selected from H, F, Cl, methyl or methyl ester, and n1 and n2 are each independently 0, 1 or 2.
5. The pre-lithiation binder according to any one of claims 1 to 4, It is characterized in that The pre-lithiation binder is selected from one or more of the following structures:
6. The pre-lithiation binder according to any one of claims 1 to 5, It is characterized in that The pre-lithiation binder is selected from any two of the following structures: Preferably, the pre-lithiation binder is: And x+y=n, x:y=0.8~1.
2.
7. A method for preparing the pre-lithiation binder according to any one of claims 1 to 6, It is characterized in that The preparation method comprises: Step S1, preparing polybiphenyl acrylate; Step S2, preparing a lithium-containing organic solution; Step S3, adding the polybiphenyl acrylate to the lithium-containing organic solution to react to obtain the pre-lithiation binder; The structure of the polybiphenyl acrylate is:
8. The preparation method according to claim 7, It is characterized in that The molar ratio of the lithium to the polybiphenyl acrylate is (1.1-1.5):1; Preferably, the reaction time is 1 to 3 hours, and the reaction is carried out under the protection of nitrogen and / or argon.
9. The preparation method according to claim 7 or 8, It is characterized in that The reaction temperature is 25±2° C., and the solvent used to prepare the organic solution is tetrahydrofuran.
10. A lithium ion battery separator, comprising a base film and a coating disposed on one surface of the base film, It is characterized in that The coating layer comprises the pre-lithiation binder according to any one of claims 1 to 6.
11. The lithium ion battery separator according to claim 10, It is characterized in that Based on the total weight of the coating being 100%, the weight of the pre-lithiation binder accounts for 10% to 40%; Preferably, the thickness of the coating is 1 μm to 3 μm, and the number of the coating is 1 or 2 layers.
12. A lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the negative electrode sheet comprises a negative electrode current collector and a negative electrode active layer disposed on at least one side surface of the negative electrode current collector, the positive electrode sheet comprises a positive electrode current collector and a positive electrode active layer disposed on at least one side surface of the positive electrode current collector, and the separator is disposed between the negative electrode active layer of the negative electrode sheet and the positive electrode active layer of the positive electrode sheet, It is characterized in that The separator is the lithium-ion battery separator according to claim 10 or 11, and the coating layer of the lithium-ion battery separator is arranged in contact with the negative electrode active layer.