Flame-retardant polyurethane composite material and preparation method thereof

By using a composite of nano-magnesium hydroxide aluminum hydroxide and a hydroxyl-containing coupling agent in polyurethane sealant, combined with toluene-3,5-diisocyanate crosslinking technology, the flame retardant and antibacterial properties of polyurethane sealant in kitchen environment are solved. The problem of this achieves better flame retardant and antibacterial effects.

CN119081626APending Publication Date: 2024-12-06LISHUI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411123788.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing polyurethane sealants are difficult to have excellent flame retardant and antibacterial properties in kitchen environments, especially when oils are attached, they are prone to bacterial growth.

Method used

Nanomagnesium hydroxide is used as an antibacterial flame retardant, and crosslinked with toluene-3,5-diisocyanate through a complex containing hydroxyl coupling agent and antibacterial agent to form a network structure of mutual crosslinking to improve the flame retardant type Flame retardant and antibacterial properties of polyurethane composites.

Benefits of technology

It significantly improves the flame retardant properties and antibacterial long-term performance of polyurethane composites, enhances its waterproof, fire-proof and mildew-proof properties in kitchen environments, and avoids the operational complexity of finding flame retardants and antibacterial agents alone.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004995791520000091
    Figure BDA0004995791520000091
  • Figure BDA0004995791520000101
    Figure BDA0004995791520000101
  • Figure BDA0004995791520000111
    Figure BDA0004995791520000111
Patent Text Reader

Abstract

The invention relates to the technical field of household furniture auxiliary materials, in particular to a flame-retardant polyurethane composite material and a preparation method thereof. The flame-retardant polyurethane composite material is formed by mixing a component A and a component B, and the mass ratio of the component A to the component B is 1: (1-6); the component A is a polyurethane prepolymer; the component B comprises the following raw materials in parts by mass: 20-30 parts of polyether polyol, 2-8 parts of a plasticizer, 30-50 parts of an antibacterial flame retardant, 1-2 parts of a catalyst and 1-2 parts of a thixotropic agent; the antibacterial flame retardant is a complex of nano magnesium aluminum hydroxide subjected to surface modification by a hydroxyl-containing coupling agent, a hydroxyl-containing antibacterial agent and toluene-3, 5-diisocyanate. The flame-retardant polyurethane composite material disclosed by the invention has excellent flame retardant property and antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of household furniture auxiliary materials, and more specifically, to a flame-retardant polyurethane composite material and a preparation method thereof. Background Art

[0002] Sealant is an organic material used to fill gaps, holes, joints or seams, which mainly includes silicone sealants, polyurethane sealants, acrylic sealants, SBR rubber sealants, etc. Among them, polyurethane sealants have good comprehensive performance and moderate prices, so they are widely used in the field of home furniture.

[0003] In the kitchen, polyurethane sealants are usually used on cabinets and sinks for aesthetics and waterproofing. However, due to the characteristics of the kitchen, there are open flames and grease adhesion, and grease adhesion will lead to the growth of mold. Therefore, higher requirements are put forward for polyurethane sealants currently used in kitchens, that is, a polyurethane sealant with excellent flame retardant and antibacterial properties is urgently needed. Summary of the invention

[0004] In order to improve the defect that conventional polyurethane sealants are difficult to have both flame retardant properties and antibacterial properties, the present application provides a flame retardant polyurethane composite material and a preparation method thereof.

[0005] In a first aspect, the present application provides a flame retardant polyurethane composite material, which adopts the following technical solution:

[0006] A flame retardant polyurethane composite material, the flame retardant polyurethane composite material is formed by mixing component A and component B, the mass ratio of component A to component B is 1:(1-6);

[0007] The component A is a polyurethane prepolymer;

[0008] The B component includes the following raw materials in parts by weight:

[0009] 20-30 parts of polyether polyol, 2-8 parts of plasticizer, 30-50 parts of antibacterial flame retardant, 1-2 parts of catalyst and 1-2 parts of thixotropic agent;

[0010] The antibacterial flame retardant is a complex of nano magnesium aluminum hydroxide surface-modified by a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate.

[0011] Magnesium aluminum hydroxide, also known as hydrotalcite, has a variety of inorganic metal ions, such as Mg 2+ 、Al 3+ , and also has OH - and H 2O, therefore, magnesium aluminum hydroxide has the same flame retardant and filling effects as aluminum hydroxide or magnesium hydroxide, and even has a more prominent flame retardant effect due to the diversity of ions.

[0012] At the same time, since magnesium aluminum hydroxide is also an insoluble substance, its compatibility with the polyurethane sealant matrix is ​​poor. Nano-sizing magnesium aluminum hydroxide can effectively reduce the particle size of magnesium aluminum hydroxide, thereby improving the compatibility of magnesium aluminum hydroxide with polyurethane sealant.

[0013] In order to further improve the compatibility of magnesium aluminum hydroxide and polyurethane sealant, in the present application, the surface of nano magnesium aluminum hydroxide is modified by a coupling agent, and the flame-retardant polyurethane composite material is made to finally exhibit better flame retardant properties.

[0014] As for the use of antimicrobial agents, when granular antimicrobial agents are selected, the antimicrobial agents tend to settle slowly, while when liquid antimicrobial agents are selected, the antimicrobial agents tend to migrate out, thereby affecting the long-term antimicrobial effect of the antimicrobial agents.

[0015] In the present application, a hydroxyl-containing coupling agent and a hydroxyl-containing antibacterial agent are selected, and then toluene-3,5-diisocyanate is added. The two isocyanates on the toluene-3,5-diisocyanate are respectively connected to the two hydroxyl groups on the coupling agent and the antibacterial agent, thereby forming a mutually cross-linked complex network, thereby effectively reducing the possibility of deviation or precipitation of the flame retardant and the antibacterial agent, and indirectly improving the long-term antibacterial performance and flame retardant performance of the flame-retardant polyurethane composite material.

[0016] At the same time, antibacterial flame retardants can have both flame retardant and antibacterial effects, eliminating the need to search for flame retardants and antibacterial agents separately.

[0017] Preferably, the hydroxyl-containing coupling agent is one or a mixture of 2-hydroxyethyl methacrylate phosphate, 3-aminopropyl trihydroxysilane and hydroxyethyl ethylenediamine triacetic acid.

[0018] Preferably, the hydroxyl-containing coupling agent is a mixture of 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxy silane, and the molar ratio of 2-hydroxyethyl methacrylate phosphate to 3-aminopropyl trihydroxy silane is (2-4):1.

[0019] 2-Hydroxyethyl methacrylate phosphate is a phosphorus coupling agent. Since it contains a phosphate system, it can also be used as an organic phosphorus flame retardant. 3-Aminopropyl trihydroxysilane contains propylamino groups, so it can also be used as a nitrogen-based flame retardant, thereby enabling flame-retardant polyurethane composite materials to have better flame retardant properties.

[0020] Compared with the use of 2-hydroxyethyl methacrylate phosphate or 3-aminopropyl trihydroxysilane alone, when 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxysilane are used in combination, especially when the molar ratio of 2-hydroxyethyl methacrylate phosphate to 3-aminopropyl trihydroxysilane is (2-4):1, the two can form a phosphorus-nitrogen synergistic flame retardant, thereby further improving the flame retardant properties of the flame-retardant polyurethane composite material.

[0021] In addition, when 2-hydroxyethyl methacrylate phosphate, 3-aminopropyl trihydroxysilane and nano magnesium aluminum hydroxide are used in combination, the metal oxides produced by the decomposition of magnesium aluminum hydroxide can also absorb a small amount of toxic / corrosive gases produced by heating 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxysilane, thereby effectively reducing the impact of combustion gases on people's bodies.

[0022] Preferably, the preparation method of the surface-modified nano magnesium aluminum hydroxide containing a hydroxyl coupling agent comprises the following steps:

[0023] Preparation of nano magnesium aluminum hydroxide solution:

[0024] Mg(NO) 2 6H 2 O and Al(NO) 3 9H 2 O is dissolved in water in a mass ratio of (3-5): (2-4) to prepare a mixed salt solution;

[0025] NaOH and Na 2 CO 3 Dissolve in water in a mass ratio of (2-4):1 to prepare a mixed alkali solution;

[0026] The mixed salt solution and the mixed alkali solution are added dropwise to water at the same addition rate, and then a NaOH solution is added dropwise to adjust the pH value to alkaline until the mixed salt solution and the mixed alkali solution are added dropwise to obtain a nano-magnesium aluminum hydroxide solution;

[0027] Nano-magnesium hydroxide aluminum modification:

[0028] The nano magnesium aluminum hydroxide solution is heated to 60-70° C., and then a hydroxyl-containing coupling agent is added dropwise, wherein the amount of the hydroxyl-containing coupling agent added is 20-30% of the total mass of the nano magnesium aluminum hydroxide solution. The solution is stirred at a constant temperature for 2-3 hours, then allowed to stand for 15-20 hours, and finally cooled, filtered, washed, and dried to obtain nano magnesium aluminum hydroxide surface-modified with a hydroxyl-containing coupling agent.

[0029] Preferably, the hydroxyl-containing antibacterial agent comprises the following raw materials: dimethyl sulfoxide, dichloromethane, catechol, sodium hydroxide, azobisisobutyronitrile, N-chlorosuccinimide, carbon tetrachloride, 2,2,6,6-tetramethylpiperidinol and sodium hypochlorite.

[0030] Preferably, the preparation method of the hydroxyl-containing antibacterial agent comprises the following steps:

[0031] S1, dimethyl sulfoxide and dichloromethane are mixed, and then catechol and sodium hydroxide solution are added in sequence at a temperature of 100-120° C., and the reaction is carried out for 1-3 hours to obtain intermediate 1;

[0032] S2, mixing intermediate 1, azobisisobutyronitrile, N-chlorosuccinimide and carbon tetrachloride, reflux reaction at 80-100° C. for 2-3 hours, introducing chlorine gas, and reacting under light conditions for 5-8 hours to obtain intermediate 2;

[0033] S3, dissolving the intermediate 2 in tetrahydrofuran, then adding 2,2,6,6-tetramethylpiperidinol at a temperature of 40-60° C., adjusting the pH value of the mixture to 8 with sodium carbonate, and continuing the reaction for 2-3 hours to obtain the intermediate 3;

[0034] S4, adding intermediate 3 to a sodium hypochlorite solution, stirring at a temperature of 40-60° C. for 2-3 h to obtain intermediate 4;

[0035] S5. Mix the intermediate 4, deionized water, ethanol and sodium borohydride, react at a temperature of 30-40° C. for 0.5-1 h, and finally remove the solvent by distillation to obtain a hydroxyl-containing antibacterial agent.

[0036] Preferably, the usage ratio of dimethyl sulfoxide, dichloromethane, catechol and sodium hydroxide solution is 100-140ml:60-80ml:0.1-0.3mol:90-110ml; the mass fraction of the sodium hydroxide solution is 45%;

[0037] and / or;

[0038] The usage ratio of the intermediate 1, azobisisobutyronitrile, N-chlorosuccinimide, carbon tetrachloride and chlorine is 20-30mmol: 0.04-0.06g: 6-8g: 50-70ml: 10-20mmol;

[0039] and / or;

[0040] The molar ratio of the intermediate 2 to 2,2,6,6-tetramethylpiperidinol is 1:(1.5-2.5);

[0041] and / or;

[0042] The dosage ratio of the intermediate 3 and the sodium hypochlorite solution is 1g:5-15ml, and the mass fraction of the sodium hypochlorite solution is 10%;

[0043] and / or;

[0044] The usage ratio of the intermediate 4, deionized water, ethanol and sodium borohydride is 4-6mmol:2-4ml:15-25ml:8-12mmol.

[0045] Preferably, the preparation method of the antibacterial flame retardant is:

[0046] Nano magnesium aluminum hydroxide surface modified with a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent, toluene-3,5-diisocyanate and N,N-dimethylformamide are mixed, wherein the molar ratio of the hydroxyl coupling agent, the hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate is 1:1:1, and then dibutyltin dilaurate is added at 60-80°C, reacted for 6-8h, and finally the solvent is evaporated to obtain an antibacterial flame retardant.

[0047] Preferably, the flame retardant polyurethane composite material is formed by mixing component A and component B, and the mass ratio of component A to component B is 1:(1-6);

[0048] The A component is an MDI prepolymer;

[0049] The B component includes the following raw materials in parts by weight:

[0050] 20-30 parts of polytetrahydrofuran, 2-8 parts of glycol benzoate, 30-50 parts of antibacterial flame retardant, 1-2 parts of stannous octoate and 1-2 parts of polyamide;

[0051] The antibacterial flame retardant is a complex of nano magnesium aluminum hydroxide surface-modified by a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate.

[0052] In a second aspect, the present application provides a method for preparing a flame-retardant polyurethane composite material, using the following technical solution:

[0053] A method for preparing a flame retardant polyurethane composite material comprises the following steps:

[0054] Step 1: Mix, disperse and degas the polyether polyol, plasticizer, antibacterial flame retardant, catalyst and thixotropic agent to obtain component B;

[0055] Step 2: Mix component A and component B for standby use to obtain a flame retardant polyurethane composite material.

[0056] In summary, this application has the following beneficial effects:

[0057] 1. Magnesium aluminum hydroxide, also known as hydrotalcite, contains a variety of inorganic metal ions, such as Mg 2+ 、Al 3+ , and also has OH - and H 2 O, therefore, magnesium aluminum hydroxide has the same flame retardant and filling effects as aluminum hydroxide or magnesium hydroxide, and even has a more prominent flame retardant effect due to the diversity of ions.

[0058] 2. Since magnesium aluminum hydroxide is also an insoluble substance, its compatibility with the polyurethane sealant matrix is ​​poor. Nano-magnesium aluminum hydroxide can effectively reduce the particle size of magnesium aluminum hydroxide, thereby improving the compatibility of magnesium aluminum hydroxide with polyurethane sealant. At the same time, the surface of nano magnesium aluminum hydroxide is modified by coupling agent, and the flame-retardant polyurethane composite material is finally made to show better flame retardant properties.

[0059] 3. In the present application, a hydroxyl-containing coupling agent and a hydroxyl-containing antibacterial agent are selected, and then toluene-3,5-diisocyanate is added. The two isocyanates on toluene-3,5-diisocyanate are respectively connected to the two hydroxyl groups on the coupling agent and the antibacterial agent, thereby forming a complex cross-linked network, thereby effectively reducing the possibility of displacement or precipitation of the flame retardant and the antibacterial agent, and indirectly improving the long-term antibacterial performance and flame retardant properties of the flame-retardant polyurethane composite material. DETAILED DESCRIPTION

[0060] The present application is further described in detail below in conjunction with Examples 1-8 and Comparative Examples 1-5.

[0061] raw material

[0062] Polyurethane prepolymer MDI prepolymer Wengjiang reagent; Toluene-3,5-diisocyanate CAS: 54132-75-1; 2-Hydroxyethyl methacrylate phosphate CAS: 52628-03-2; 3-Aminopropyl trihydroxysilane CAS: 58160-99-9; Hydroxyethylethylenediaminetriacetic acid CAS: 150-39-0; Mg(NO) 2 6H 2 OCAS: 10377-60-3; Al(NO) 3 9H 2 O CAS: 13473-90-0; NaOH CAS: 1310-73-2; Na 2 CO 3CAS: 497-19-8; Dimethyl sulfoxide CAS: 67-68-5; Dichloromethane CAS: 75-09-2; Catechol CAS: 120-80-9; Azobisisobutyronitrile CAS: 78-67-1; N-chlorosuccinimide CAS: 128-09-6; Carbon tetrachloride CAS: 56-23-5; 2,2,6,6-tetramethylpiperidinol CAS: 2403-88-5; Sodium hypochlorite CAS: 7681-52-9; Sodium borohydride CAS: 16940-66-2; Dibutyltin dilaurate CAS: 77-58-7; Polytetrahydrofuran CAS: 25190-06-1; Diol benzoate CAS: 20587-61-5; Stannous octoate CAS: 301-10-0;

[0063] Polyamide CAS: 63428-84-2.

[0064] Example

[0065] Example 1

[0066] A flame retardant polyurethane composite material, which is mixed with component A and component B, and the mass ratio of component A to component B is 1:4;

[0067] Component A is polyurethane prepolymer-MDI prepolymer;

[0068] Component B includes the following raw materials: polyether polyol-polytetrahydrofuran 25g, plasticizer-benzoic acid glycol ester 5g, antibacterial flame retardant 40g, catalyst-stannous octoate 1.5g and thixotropic agent-polyamide 1.5g.

[0069] The antibacterial flame retardant is a complex of nano magnesium aluminum hydroxide surface-modified with a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate.

[0070] Specifically, the preparation method of nano magnesium aluminum hydroxide surface modified by a hydroxyl coupling agent comprises the following steps:

[0071] Preparation of nano magnesium aluminum hydroxide solution:

[0072] Mg(NO) 2 6H 2 O and Al(NO) 3 9H 2 O is dissolved in water in a mass ratio of 4:3 to prepare a mixed salt solution;

[0073] NaOH and Na 2 CO 3 Dissolve in water at a mass ratio of 3:1 to prepare a mixed alkali solution;

[0074] The mixed salt solution and the mixed alkali solution are added dropwise to water at the same addition rate, and then a NaOH solution is added dropwise to adjust the pH value to alkaline until the mixed salt solution and the mixed alkali solution are added dropwise to obtain a nano-magnesium aluminum hydroxide solution;

[0075] Nano-magnesium hydroxide aluminum modification:

[0076] The nano magnesium aluminum hydroxide solution was heated to 65°C, and then a hydroxyl-containing coupling agent was added dropwise, wherein the amount of the hydroxyl-containing coupling agent added was 25% of the total mass of the nano magnesium aluminum hydroxide solution, and the mixture was stirred at a constant temperature for 3 hours, and then allowed to stand for 18 hours, and finally cooled, filtered, washed, and dried to obtain nano magnesium aluminum hydroxide surface-modified with a hydroxyl-containing coupling agent;

[0077] The hydroxyl-containing coupling agent is 2-hydroxyethyl methacrylate phosphate.

[0078] The preparation method of the hydroxyl-containing antibacterial agent comprises the following steps:

[0079] S1, dimethyl sulfoxide and dichloromethane are mixed, and then catechol and sodium hydroxide solution are added in sequence at a temperature of 110° C. and reacted for 2 hours to obtain intermediate 1;

[0080] The dosage ratio of dimethyl sulfoxide, dichloromethane, catechol and sodium hydroxide solution is 120ml:70ml:0.2mol:100ml; the mass fraction of sodium hydroxide solution is 45%;

[0081] S2, mixing intermediate 1, azobisisobutyronitrile, N-chlorosuccinimide and carbon tetrachloride, reflux at 90°C for 3h, introducing chlorine gas, and reacting under light conditions for 6h to obtain intermediate 2;

[0082] The ratio of intermediate 1, azobisisobutyronitrile, N-chlorosuccinimide, carbon tetrachloride and chlorine is 25mmol:0.05g:7g:60ml:15mmol;

[0083] S3, dissolving the intermediate 2 in tetrahydrofuran, then adding 2,2,6,6-tetramethylpiperidinol at a temperature of 50° C., adjusting the pH value of the mixed solution to 8 with sodium carbonate, and continuing the reaction for 3 h to obtain the intermediate 3;

[0084] The molar ratio of intermediate 2 and 2,2,6,6-tetramethylpiperidinol is 1:2, and the amount of tetrahydrofuran is excessive;

[0085] S4, adding intermediate 3 to a sodium hypochlorite solution, stirring at 50° C. for 3 h to obtain intermediate 4;

[0086] The dosage ratio of intermediate 3 and sodium hypochlorite solution is 1g:10ml, and the mass fraction of sodium hypochlorite solution is 10%;

[0087] S5, mixing the intermediate 4, deionized water, ethanol and sodium borohydride, reacting at 35° C. for 1 h, and finally distilling off the solvent to obtain a hydroxyl-containing antibacterial agent;

[0088] The usage ratio of intermediate 4, deionized water, ethanol and sodium borohydride is 5mmol:3ml:20ml:10mmol.

[0089] The preparation method of the antibacterial flame retardant is as follows:

[0090] Nano magnesium aluminum hydroxide surface modified with a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent, toluene-3,5-diisocyanate and N,N-dimethylformamide are mixed, wherein the molar ratio of the hydroxyl coupling agent, the hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate is 1:1:1, and N,N-dimethylformamide is excessive. Subsequently, dibutyltin dilaurate is added at 70° C., and the addition amount of dibutyltin dilaurate is 2% of the total mass. The reaction is carried out for 7 hours, and finally the solvent is evaporated to obtain an antibacterial flame retardant.

[0091] The preparation method of the flame retardant polyurethane composite material comprises the following steps:

[0092] Step 1: Mix, disperse and degas the polyether polyol, plasticizer, antibacterial flame retardant, catalyst and thixotropic agent to obtain component B;

[0093] Step 2: Mix component A and component B for standby use to obtain a flame retardant polyurethane composite material.

[0094] Example 2-3

[0095] The difference from Example 1 is that the addition amounts of the components of the flame retardant polyurethane composite material are different, as shown in Table 1.

[0096] Table 1 Addition amount of each component of the flame retardant polyurethane composite material in Examples 1-3

[0097]

[0098]

[0099] Example 4

[0100] The difference from Example 1 is that 2-hydroxyethyl methacrylate phosphate is replaced by the same molar amount of 3-aminopropyltrihydroxysilane.

[0101] Example 5

[0102] The difference from Example 1 is that 2-hydroxyethyl methacrylate phosphate is replaced by the same molar amount of hydroxyethyl ethylenediamine triacetic acid.

[0103] Example 6

[0104] The difference from Example 1 is that 2-hydroxyethyl methacrylate phosphate is replaced by a mixture of 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxysilane in the same molar amount, and the molar ratio of 2-hydroxyethyl methacrylate phosphate to 3-aminopropyl trihydroxysilane is 3:1.

[0105] Example 7

[0106] The difference from Example 1 is that 2-hydroxyethyl methacrylate phosphate is replaced by a mixture of 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxysilane in the same molar amount, and the molar ratio of 2-hydroxyethyl methacrylate phosphate to 3-aminopropyl trihydroxysilane is 2:1.

[0107] Example 8

[0108] The difference from Example 1 is that 2-hydroxyethyl methacrylate phosphate is replaced by a mixture of 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxysilane in the same molar amount, and the molar ratio of 2-hydroxyethyl methacrylate phosphate to 3-aminopropyl trihydroxysilane is 4:1.

[0109] Comparative Example

[0110] Comparative Example 1

[0111] The difference from Example 1 is that no antibacterial flame retardant is added.

[0112] Comparative Example 2

[0113] The difference from Example 1 is that the nano magnesium aluminum hydroxide surface-modified by a hydroxyl-containing coupling agent is no longer added.

[0114] Comparative Example 3

[0115] The difference from Example 1 is that the surface of nano-magnesium aluminum hydroxide is no longer modified by a hydroxyl-containing coupling agent.

[0116] Comparative Example 4

[0117] The difference from Example 6 is that no hydroxyl-containing antibacterial agent is added.

[0118] Comparative Example 5

[0119] The difference from Example 6 is that toluene-3,5-diisocyanate is not added.

[0120] Performance testing

[0121] Detection Methods

[0122] 1. Flame retardant performance test

[0123] Three samples were taken out from Examples 1-8, Comparative Examples 1-3 and Comparative Example 5 respectively and cured into strips, and then the flame retardant properties of the samples were tested with reference to GB / T2406-93 "Plastics - Determination of flammability by oxygen index method", and then the oxygen index was obtained and the average value was taken.

[0124] The test data are shown in Table 2.

[0125] Table 2 Flame retardant performance test table of Examples 1-8 and Comparative Examples 1-3

[0126]

[0127]

[0128] 2. Antibacterial performance test

[0129] Three samples were taken from Example 1 and Comparative Examples 4-5, respectively, and solidified into sheets. Then, they were immersed in 100 mL of 10 5 The mold spore suspension AS3.3928, with a material concentration of 1.25 mg / mL, was incubated at 37°C in a constant temperature shaker at 200 rpm for 3 h. 100 μL of the supernatant was taken in a culture dish to observe the bacterial growth, and the antibacterial activity of the sample was tested again after one year of use.

[0130] The test results are shown in Table 3.

[0131] Table 3 Antibacterial performance of Example 1 and Comparative Examples 4-5

[0132] Example 6 Comparative Example 4 Comparative Example 5 Antimicrobial No bacteria found Full of bacteria No bacteria found Antibacterial activity after one year No bacteria found Full of bacteria A small amount of bacteria

[0133] Referring to Example 1 and Comparative Example 1 and combining with Table 2, it can be seen that the oxygen index of Comparative Example 1 is significantly reduced compared with that of Example 1, which indicates that the addition of the antibacterial flame retardant can effectively improve the flame retardant properties of the flame retardant polyurethane composite material.

[0134] Referring to Example 1 and Comparative Example 2 and in combination with Table 2, it can be seen that relative to Example 1, the oxygen index of Comparative Example 2 is significantly reduced, and even the oxygen index of Comparative Example 2 is extremely similar to that of Comparative Example 1, which shows that the addition of nano-magnesium aluminum hydroxide surface-modified with a hydroxyl coupling agent can effectively improve the flame retardant properties of the flame-retardant polyurethane composite material.

[0135] Referring to Example 1 and Comparative Examples 2-3 and in combination with Table 2, it can be seen that relative to Example 1, the oxygen index of Comparative Example 3 is significantly reduced, but relative to Comparative Example 2, the oxygen index of Comparative Example 3 is relatively improved, which shows that the addition of nano-magnesium aluminum hydroxide can effectively improve the flame retardant properties of the flame-retardant polyurethane composite material, and the modification of the surface of nano-magnesium aluminum hydroxide with a hydroxyl coupling agent can further improve the flame retardant properties of the flame retardant polyurethane composite material.

[0136] The reason is that magnesium aluminum hydroxide, also known as hydrotalcite, contains a variety of inorganic metal ions, such as Mg 2+ 、Al 3+ , and also has OH - and H 2 O, therefore, magnesium aluminum hydroxide has the same flame retardant and filling effects as aluminum hydroxide or magnesium hydroxide, and even has a more prominent flame retardant effect due to the diversity of ions.

[0137] In addition, since magnesium aluminum hydroxide is also an insoluble substance, its compatibility with the polyurethane sealant matrix is ​​poor. Nano-sizing magnesium aluminum hydroxide can effectively reduce the particle size of magnesium aluminum hydroxide, thereby improving the compatibility of magnesium aluminum hydroxide with polyurethane sealant. At the same time, the surface of nano magnesium aluminum hydroxide is modified with a coupling agent, and the flame-retardant polyurethane composite material is finally exhibited with better flame retardant properties.

[0138] Referring to Examples 1-3 and in combination with Table 2, it can be seen that the oxygen index of Examples 2-3 is slightly lower than that of Example 1, which indicates that when the components of the flame-retardant polyurethane composite material are added in the amounts of Example 1, the prepared flame-retardant polyurethane composite material will have better flame retardant properties.

[0139] With reference to Example 1 and Examples 4-5 and in combination with Table 2, it can be seen that, relative to Example 1, the oxygen index of Example 4 is slightly decreased, while the oxygen index of Example 5 is further decreased, which indicates that, relative to the use of hydroxyethylethylenediaminetriacetic acid, the use of 2-hydroxyethyl methacrylate phosphate and 3-aminopropyltrihydroxysilane can promote the flame retardant polyurethane composite material to have better flame retardant properties.

[0140] The reason is that hydroxyethyl methacrylate phosphate is a phosphorus coupling agent. Since it contains a phosphate system, it can also be used as an organic phosphorus flame retardant. 3-aminopropyltrihydroxysilane contains propylamino groups, so it can also be used as a nitrogen-based flame retardant, thereby enabling the flame-retardant polyurethane composite material to have better flame retardant properties.

[0141] Referring to Example 1, Example 4 and Examples 6-8 and combining with Table 2, it can be seen that compared with Example 1 and Example 4, the oxygen index of Examples 6-8 is significantly improved, which shows that compared with the use of 2-hydroxyethyl methacrylate phosphate or 3-aminopropyl trihydroxysilane alone, when 2-hydroxyethyl methacrylate phosphate is used in combination with 3-aminopropyl trihydroxysilane, the two can form a phosphorus-nitrogen synergistic flame retardant, thereby further improving the flame retardant properties of the flame-retardant polyurethane composite material.

[0142] Compared with Example 6, the oxygen index of Examples 7-8 is relatively low, which shows that when 2-hydroxyethyl methacrylate phosphate or 3-aminopropyl trihydroxysilane adopts the molar ratio of Example 6, the prepared flame-retardant polyurethane composite material will have better flame retardant properties.

[0143] Referring to Example 6 and Comparative Examples 4-5 and in combination with Tables 2-3, it can be seen that the antibacterial performance of Comparative Example 4 is significantly reduced compared with that of Example 6, which indicates that the hydroxyl-containing antibacterial agent has excellent antibacterial performance.

[0144] Compared with Example 6, the oxygen index of Example 5 is significantly reduced, and the antibacterial property of Example 5 is also significantly reduced, which shows that the addition of toluene-3,5-diisocyanate can improve the flame retardant and antibacterial properties of the flame retardant polyurethane composite material to a certain extent.

[0145] The reason is that when using antimicrobial agents, granular antimicrobial agents tend to settle slowly, while liquid antimicrobial agents tend to migrate out, thus affecting the long-term antimicrobial effect of the antimicrobial agents. The same is true for flame retardants.

[0146] A hydroxyl-containing coupling agent and a hydroxyl-containing antibacterial agent are selected, and then toluene-3,5-diisocyanate is added. The two isocyanates on the toluene-3,5-diisocyanate are respectively connected to the two hydroxyl groups on the coupling agent and the antibacterial agent, thereby forming a complex cross-linked network, thereby effectively reducing the possibility of deviation or precipitation of the flame retardant and the antibacterial agent, and indirectly improving the long-term antibacterial performance and flame retardant performance of the flame-retardant polyurethane composite material.

[0147] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A flame retardant polyurethane composite material, characterized in that: The flame retardant polyurethane composite material is formed by mixing component A and component B, and the mass ratio of component A to component B is 1:(1-6); The component A is a polyurethane prepolymer; The B component includes the following raw materials in parts by weight: 20-30 parts of polyether polyol, 2-8 parts of plasticizer, 30-50 parts of antibacterial flame retardant, 1-2 parts of catalyst and 1-2 parts of thixotropic agent; The antibacterial flame retardant is a complex of nano magnesium aluminum hydroxide surface-modified by a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate.

2. The flame-retardant polyurethane composite material according to claim 1, characterized in that: The hydroxyl-containing coupling agent is one or a mixture of 2-hydroxyethyl methacrylate phosphate, 3-aminopropyl trihydroxysilane and hydroxyethyl ethylenediamine triacetic acid.

3. The flame retardant polyurethane composite material according to claim 2, characterized in that: The hydroxyl-containing coupling agent is a mixture of 2-hydroxyethyl methacrylate phosphate and 3-aminopropyl trihydroxy silane, and the molar ratio of 2-hydroxyethyl methacrylate phosphate to 3-aminopropyl trihydroxy silane is (2-4):

1.

4. The flame-retardant polyurethane composite material according to claim 1, characterized in that: The preparation method of the surface-modified nano magnesium aluminum hydroxide containing a hydroxyl coupling agent comprises the following steps: Preparation of nano magnesium aluminum hydroxide solution: Dissolve Mg(NO)2·6H2O and Al(NO)3·9H2O in water in a mass ratio of (3-5):(2-4) to prepare a mixed salt solution; Dissolve NaOH and Na2CO3 in water in a mass ratio of (2-4):1 to prepare a mixed alkaline solution; The mixed salt solution and the mixed alkali solution are added dropwise to water at the same addition rate, and then a NaOH solution is added dropwise to adjust the pH value to alkaline until the mixed salt solution and the mixed alkali solution are added dropwise to obtain a nano-magnesium aluminum hydroxide solution; Nano-magnesium hydroxide aluminum modification: The nano magnesium aluminum hydroxide solution is heated to 60-70° C., and then a hydroxyl-containing coupling agent is added dropwise, wherein the amount of the hydroxyl-containing coupling agent added is 20-30% of the total mass of the nano magnesium aluminum hydroxide solution. The solution is stirred at a constant temperature for 2-3 hours, then allowed to stand for 15-20 hours, and finally cooled, filtered, washed, and dried to obtain nano magnesium aluminum hydroxide surface-modified with a hydroxyl-containing coupling agent.

5. The flame-retardant polyurethane composite material according to claim 1, characterized in that: The hydroxyl-containing antibacterial agent comprises the following raw materials: dimethyl sulfoxide, dichloromethane, catechol, sodium hydroxide, azobisisobutyronitrile, N-chlorosuccinimide, carbon tetrachloride, 2,2,6,6-tetramethylpiperidinol and sodium hypochlorite.

6. The flame-retardant polyurethane composite material according to claim 5, characterized in that: The preparation method of the hydroxyl-containing antibacterial agent comprises the following steps: S1, dimethyl sulfoxide and dichloromethane are mixed, and then catechol and sodium hydroxide solution are added in sequence at a temperature of 100-120° C., and the reaction is carried out for 1-3 hours to obtain intermediate 1; S2, mixing intermediate 1, azobisisobutyronitrile, N-chlorosuccinimide and carbon tetrachloride, reflux reaction at 80-100° C. for 2-3 hours, introducing chlorine gas, and reacting under light conditions for 5-8 hours to obtain intermediate 2; S3, dissolving the intermediate 2 in tetrahydrofuran, then adding 2,2,6,6-tetramethylpiperidinol at a temperature of 40-60° C., adjusting the pH value of the mixture to 8 with sodium carbonate, and continuing the reaction for 2-3 hours to obtain the intermediate 3; S4, adding intermediate 3 to a sodium hypochlorite solution, stirring at a temperature of 40-60° C. for 2-3 h to obtain intermediate 4; S5. Mix the intermediate 4, deionized water, ethanol and sodium borohydride, react at a temperature of 30-40° C. for 0.5-1 h, and finally distill off the solvent to obtain a hydroxyl-containing antibacterial agent.

7. The flame-retardant polyurethane composite material according to claim 6, characterized in that: The usage ratio of dimethyl sulfoxide, dichloromethane, catechol and sodium hydroxide solution is 100-140ml:60-80ml:0.1-0.3mol:90-110ml; the mass fraction of the sodium hydroxide solution is 45%; and / or; The usage ratio of the intermediate 1, azobisisobutyronitrile, N-chlorosuccinimide, carbon tetrachloride and chlorine is 20-30mmol: 0.04-0.06g: 6-8g: 50-70ml: 10-20mmol; and / or; The molar ratio of the intermediate 2 to 2,2,6,6-tetramethylpiperidinol is 1:(1.5-2.5); and / or; The dosage ratio of the intermediate 3 and the sodium hypochlorite solution is 1g:5-15ml, and the mass fraction of the sodium hypochlorite solution is 10%; and / or; The usage ratio of the intermediate 4, deionized water, ethanol and sodium borohydride is 4-6mmol:2-4ml:15-25ml:8-12mmol.

8. The flame-retardant polyurethane composite material according to claim 1, characterized in that: The preparation method of the antibacterial flame retardant is: Nano magnesium aluminum hydroxide surface modified with a hydroxyl coupling agent, a hydroxyl-containing antibacterial agent, toluene-3,5-diisocyanate and N,N-dimethylformamide are mixed, wherein the molar ratio of the hydroxyl coupling agent, the hydroxyl-containing antibacterial agent and toluene-3,5-diisocyanate is 1:1:1, and then dibutyltin dilaurate is added at 60-80°C, reacted for 6-8h, and finally the solvent is evaporated to obtain an antibacterial flame retardant.

9. The flame-retardant polyurethane composite material according to claim 1, characterized in that: The A component is an MDI prepolymer; The B component includes the following raw materials in parts by weight: 20-30 parts of polytetrahydrofuran, 2-8 parts of glycol benzoate, 30-50 parts of antibacterial flame retardant, 1-2 parts of stannous octoate and 1-2 parts of polyamide.

10. A method for preparing the flame-retardant polyurethane composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: Mix, disperse and degas the polyether polyol, plasticizer, antibacterial flame retardant, catalyst and thixotropic agent to obtain component B; Step 2: Mix component A and component B for standby use to obtain a flame retardant polyurethane composite material.

Citation Information

Cited By

  • High-performance flame-retardant veneer artificial board and manufacturing process thereof

    CN121105145A