Quenching buckling plate shape adjusting method
By adjusting parameters such as water ratio and roller speed according to the thickness and curvature type of the steel plate, the curvature problem before quenching of the steel plate is solved, and the flatness and hardness of the steel plate after quenching are achieved.
Patent Information
- Application Number
- CN202411228224.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-05
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
Due to the uncontrollable factors of steel rolling in the early stage, steel plates often have scoop bending before quenching, making it difficult to meet customer requirements after quenching.
According to the thickness of the steel plate, it is divided into thick plates and thin plates, and the water ratio, roller speed, roller seam height and gap nozzle water volume are adjusted according to different types of bends. For example, when the thick plate is arched in the middle, the water ratio is increased, and when the two ends are curled, the water ratio is reduced. Small water ratio, reduce the roller speed when the middle wave of the thin plate, increase the roller speed when the side wave, etc.
Through these adjustment methods, the quenched steel plate can be made to a relatively flat state, meeting customers' hardness and plate shape requirements.
Smart Images

Figure CN119082439A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel plate quenching, and in particular to a method for adjusting the shape of a quenched curved plate. Background Art
[0002] At present, the quenching process of medium and thick plates is to heat the steel plate to 900℃ and then quickly cool it through the slit nozzle of the quenching furnace to form a martensitic structure. The various parameters of the quenching furnace have been formed into process documents to ensure that the hardness and plate shape of the steel plate after quenching meet customer requirements.
[0003] Due to uncontrollable factors in the early stage of steel rolling, the steel plate often buckles before quenching. The types of steel plate buckling are mainly divided into: head (tail) buckle, head (tail warping), tail bulge, middle arch, ship shape, middle wave, side wave, etc.; if the steel plate is buckled before entering the quenching furnace, production according to the established process will result in the steel plate still being buckled after quenching. At this time, it is difficult to meet customer requirements using the original production process. Summary of the invention
[0004] The purpose of the present application includes, for example, providing a method for adjusting the shape of a quenched curved plate, which can better solve the problem of steel plate curvature.
[0005] The embodiments of the present application can be implemented as follows:
[0006] The embodiment of the present application provides a method for adjusting the shape of a quenching curved plate, which is applied to a quenching furnace. The method for adjusting the shape of a quenching curved plate includes:
[0007] According to the thickness of the steel plate, the steel plate is divided into thick plate and thin plate;
[0008] For thick plates, when the type of curvature is arched in the middle, increase the water ratio; when the type of curvature is warped at both ends, reduce the water ratio; when the type of curvature is boat-shaped throughout, increase the roller speed;
[0009] For thin plates, when the type of curvature of the thin plates is middle waves, reduce the roller speed; when the type of curvature of the thin plates is side waves, increase the roller speed; when the type of curvature of the thin plates is head buckle, increase the roller gap height; when the type of curvature of the thin plates is head warping, reduce the roller gap height; when the head section of the thin plates becomes wavy, increase the roller gap height; when the type of curvature of the thin plates is tail bulge or tail warping, increase the water volume of the gap nozzle.
[0010] Optionally, when the type of curvature of the thick plate is a boat shape, the step of increasing the roller speed includes:
[0011] For every 20mm upward tilt at both ends of the thick plate, increase the roller speed by 18 / H 2 m / s, where 18 is the empirical coefficient and H is the thickness of the steel plate in mm.
[0012] Optionally, the roller speed is increased by 18 / H for every 20mm upward tilt at both ends of the thick plate. 2 After the m / s step, it also includes:
[0013] For every 20mm upward tilt at both ends of the thick plate, increase the water volume of the gap nozzle by 30m 3 / h.
[0014] Optionally, when the type of the thin plate curvature is medium wave, the step of reducing the roller speed includes:
[0015] When the type of curvature of the thin plate is medium wave, the roller speed will be reduced by 0.05m / s for every 10mm of unevenness, and the roller gap height will be reduced by 0.5mm.
[0016] Optionally, when the type of the thin plate curvature is edge wave, the step of increasing the roller speed includes:
[0017] When the type of curvature of the thin plate is edge wave, the roller speed shall be increased by 0.05m / s for every 10mm of unevenness.
[0018] Optionally, when the type of curvature of the thin plate is edge wave, after the step of increasing the roller speed by 0.05 m / s for every 10 mm of unevenness, the method further comprises:
[0019] For every 0.05m / s increase in roller speed, increase the gap nozzle water volume by 50m 3 / h.
[0020] Optionally, when the type of the thin plate curvature is head buckle, the step of increasing the roller gap height comprises:
[0021] When the type of curvature of the thin plate is head buckle, increase the roller gap height by 0.3-1.0mm.
[0022] Optionally, when the type of the thin plate warping is head warping, the step of reducing the roller gap height includes:
[0023] When the type of warping of the thin plate is head warping, reduce the roller gap height by 0.3-1.0mm.
[0024] Optionally, when the head section of the sheet becomes corrugated, the step of increasing the roller gap height comprises:
[0025] When the head section of the thin plate becomes corrugated, the roller gap height is increased by 0.5-1.5 mm, wherein the length of the head section is 0.8-1.2 m.
[0026] Optionally, when the type of warping of the thin plate is tail bulging or tail warping, the step of increasing the water volume of the slit nozzle includes:
[0027] When the type of thin plate warping is tail bulging or tail warping, increase the gap nozzle water volume by 50m for every 10mm unevenness. 3 / h.
[0028] The beneficial effects of the plate shape adjustment method of the quenched curved plate of the embodiment of the present application include, for example: first, the steel plate is divided into thick plate and thin plate according to the thickness of the steel plate. For the thick plate, when the type of curvature of the thick plate is a middle arch, the water ratio is increased; when the type of curvature of the thick plate is warped at both ends, the water ratio is reduced; when the type of curvature of the thick plate is a whole-body boat shape, the roller speed is increased; for the thin plate, when the type of curvature of the thin plate is a middle wave, the roller speed is reduced; when the type of curvature of the thin plate is a side wave, the roller speed is increased; when the type of curvature of the thin plate is a head buckle, the roller gap height is increased; when the type of curvature of the thin plate is head warping, the roller gap height is reduced; when the head section of the thin plate becomes wavy, the roller gap height is increased; when the type of curvature of the thin plate is a tail bulge or tail warping, the water volume of the gap nozzle is increased. By taking corresponding adjustment measures for thick and thin plates according to different types of curvature, the quenched steel plate can reach a relatively flat state. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a flow chart of steps S1-S3 in the method for adjusting the shape of a quenched curved plate in an embodiment of the present application;
[0031] Figure 2 This is a flow chart of sub-steps S21-S22 in the method for adjusting the shape of a quenched curved plate in an embodiment of the present application;
[0032] Figure 3 This is a flow chart of sub-steps S31-S33 in the method for adjusting the shape of a quenched curved plate in an embodiment of the present application;
[0033] Figure 4 This is a flow chart of sub-steps S34-S37 in the method for adjusting the shape of a quenched curved plate in an embodiment of the present application. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0035] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0036] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0037] In the description of the present application, it should be noted that if the terms "upper", "lower", "inside", "outside", etc. appear to indicate an orientation or position relationship, it is based on the orientation or position relationship shown in the drawings, or is the orientation or position relationship in which the product of the invention is usually placed when used. It is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0038] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.
[0039] It should be noted that, in the absence of conflict, the features in the embodiments of the present application may be combined with each other.
[0040] The inventor of this application found that due to uncontrollable factors in the early stage of steel rolling, the steel plate often buckles before quenching. The types of steel plate buckling are mainly divided into: head (tail) buckle, head (tail) warping, tail bulge, middle arch, boat shape, middle wave, side wave, etc. If the steel plate is buckled before entering the quenching furnace, the production according to the established process will cause the steel plate to still be buckled after quenching. At this time, it is difficult to meet customer requirements using the original production process. The embodiment of this application provides a method for adjusting the shape of a quenched buckled plate, which is at least used to solve this technical problem.
[0041] Please refer to Figure 1-Figure 4 The quenching plate shape adjustment method provided in the embodiment of the present application is applied to a quenching furnace. The main process parameters of the quenching furnace include: water volume, water ratio (the ratio of the water volume of the lower nozzle to the water volume of the upper nozzle), roll gap height, and roll speed.
[0042] Since the type and degree of warping of the same batch of steel plates before entering the quenching furnace are often the same, by observing the plate shape before entering the furnace and uniformly changing the process parameters, a batch of steel plates that may have warped after quenching can be made flat.
[0043] Specifically, the plate shape adjustment method includes:
[0044] Step S1, dividing the steel plates into thick plates and thin plates according to their thickness.
[0045] In this embodiment, a steel plate with a thickness less than 16 mm is classified as a thin plate, and a steel plate with a thickness greater than or equal to 16 mm is classified as a thick plate.
[0046] For thick plates, the phase change stress is mainly considered, which conforms to the law of "cold expansion and thermal contraction"; for thin plates, the thermal stress is mainly considered, which conforms to the law of "thermal expansion and thermal contraction". The principle is that the cooling capacity of thin plates is strong, and the upper and lower surfaces and the core undergo phase change at almost the same time, so the phase change stress of the steel plate has little effect at this time. The phase change of the upper surface, core, and lower surface of thick plates cannot occur at the same time, so the phase change stress has a greater impact and is greater than the thermal stress.
[0047] Due to the above reasons, the water ratio and roller speed are mainly considered when adjusting the plate shape of thick plates, because the water ratio directly affects the difference in cooling speed between the upper and lower surfaces of the steel plate, and the roller speed directly affects the difference in cooling speed between the inner and outer layers of the steel plate. When adjusting thin plates, the roller speed, roller gap height, and the amount of water in the gap nozzle are mainly considered. The roller speed mainly considers whether the water on the upper surface of the steel plate can be discharged in time, which affects the changes in the cooling speed of the middle and edge parts; because the supporting force of thin plates is relatively small, the roller gap mainly affects the pressing force when the steel plate enters the quenching furnace, and the water volume mainly affects the overall cooling speed of the steel plate.
[0048] Step S2, for thick plates, when the type of curvature of the thick plates is arched in the middle, increase the water ratio; when the type of curvature of the thick plates is warped at both ends, reduce the water ratio; when the type of curvature of the thick plates is boat-shaped throughout, increase the roller speed.
[0049] Among them, when the type of curvature of the thick plate is arched in the middle, the water ratio is increased by 0.1-0.2; when the type of curvature of the thick plate is warped at both ends, the water ratio is reduced by 0.1-0.2; the minimum value of the water ratio after adjustment shall not be less than 1.0, and the maximum value shall not be greater than 1.5. If the water ratio is less than 1.0, the water volume of the lower nozzle is small, which reduces the cooling capacity of the lower surface of the steel plate, resulting in insufficient martensiticization, and further reduces the hardness of the lower surface of the steel plate; if the water ratio is greater than 1.5, the total water volume is large, which will cause the water pump power to increase, and the pump may burn out.
[0050] Step S3, for the thin plate, when the type of curvature of the thin plate is middle wave, reduce the roller speed; when the type of curvature of the thin plate is side wave, increase the roller speed; when the type of curvature of the thin plate is head buckle, increase the roller gap height; when the type of curvature of the thin plate is head warping, reduce the roller gap height; when the head section of the thin plate becomes wavy, increase the roller gap height; when the type of curvature of the thin plate is tail bulge or tail warping, increase the water volume of the gap nozzle.
[0051] It should be noted that the wave shape before the thin plate enters the furnace has the greatest impact on the later stage, and the wave shape is the most likely plate shape problem before the heat treatment of the thin plate. The main reason for the wave shape is that the uneven pressure on the steel plate during the rolling process causes the steel plate to be subjected to different pressures at different parts, which in turn causes waves. In addition, uneven cooling of the steel plate, uneven material organization and composition may also cause waves. The wave shape is divided into middle waves and side waves. If it is a middle wave, it means that the shrinkage in the middle part of the steel plate should be increased to offset the middle wave; if it is a side wave, the shrinkage in the middle part of the steel plate should be reduced to offset the side wave.
[0052] Further, step S2 includes:
[0053] Sub-step S21: Increase the roller speed by 18 / H for every 20mm upward tilt of the two ends of the thick plate 2 m / s, where 18 is the empirical coefficient and H is the thickness of the steel plate in mm.
[0054] For example, if the thick plate is warped by 20mm at both ends and the plate thickness H is 18mm, the roller speed will be increased by 1 / 18m / s.
[0055] After sub-step S21, the method further includes:
[0056] Sub-step S22: For every 20mm upward tilt of the two ends of the thick plate, increase the water volume of the gap nozzle by 30m 3 / h.
[0057] It should be noted that, since the roller speed is increased in sub-step S21 and thick plates are not easy to be hardened, the water volume of the gap nozzle should be increased accordingly to ensure that the water volume is sufficient when the roller speed is increased.
[0058] For example, if the thick plate is tilted 40mm at both ends, increase the water volume of the gap nozzle by 60m 3 / h. If the ends of the thick plate are tilted more than 80mm, it cannot be put into the furnace for quenching. It should be flattened before quenching, otherwise the quenching furnace will be damaged.
[0059] Further, step S3 includes:
[0060] Sub-step S31, when the type of curvature of the thin plate is medium wave, the roller speed is reduced by 0.05m / s for every 10mm of unevenness, and the roller gap height is reduced by 0.5mm.
[0061] If the roller speed is reduced during quenching, the amount of water stored in the middle of the steel plate can be increased. The water cannot be discharged in time and remains in the middle of the steel plate, thereby increasing the cooling speed and shrinkage of the middle of the steel plate, thereby offsetting the middle waves.
[0062] In actual operation, a two-meter ruler is used to measure the unevenness of the steel plate (in mm). For every 10 mm of unevenness, the roller speed is reduced by 0.05 m / s. For example, for a 20 mm unevenness, the roller speed is reduced by 0.1 m / s.
[0063] When the roller speed is reduced, the head of the steel plate may be warped. At this time, the roller gap height should be reduced at the same time. The lower the roller gap height, the lower the angle of the steel plate when entering the water, so that the head of the steel plate will be lower after cooling. Specifically, the roller gap height should be reduced by 0.5mm for every 10mm unevenness. For example, for a 20mm unevenness, the roller gap height should be reduced by 1mm.
[0064] Step S3 also includes:
[0065] Sub-step S32: When the type of curvature of the thin plate is edge wave, the roller speed is increased by 0.05 m / s for every 10 mm of unevenness.
[0066] If the roller speed is increased during quenching, the amount of water in the middle of the steel plate can be reduced, and the water can be discharged from the middle of the steel plate in time, thereby reducing the cooling rate and shrinkage of the middle of the steel plate, thereby offsetting the edge waves.
[0067] In actual operation, use a two-meter ruler to measure the unevenness of the steel plate (in mm). For every 10mm of unevenness, the roller speed will be increased by 0.05m / s. For example, for a 20mm unevenness, the roller speed will be increased by 0.1m / s.
[0068] After sub-step S32, the method further includes:
[0069] Sub-step S33: For every 0.05 m / s increase in roller speed, increase the water volume of the slit nozzle by 50 m / s. 3 / h.
[0070] It should be noted that when the type of thin plate curvature is edge wave and the roller speed is increased, the cooling rate of the steel plate will decrease accordingly. At this time, the water volume of the gap nozzle should be increased to ensure that the steel plate is cooled thoroughly.
[0071] For example, increase the roller speed by 0.1 m / s and increase the water volume of the slit nozzle by 100 m / s. 3 / h.
[0072] Step S3 also includes:
[0073] Sub-step S34: when the type of curvature of the thin plate is head buckle, the roller gap height is increased by 0.3-1.0 mm.
[0074] In actual operation, for thin plates with head buckle problems, raising the roller gap height by 0.3-1.0mm can effectively eliminate the head buckle problem; if the roller gap height is raised below 0.3mm, the head buckle problem may still exist, and if the roller gap height is raised to more than 1mm, the head warping problem may occur.
[0075] For example, when the type of curvature of the thin plate is head buckle, the roller gap height is increased by 0.3, 0.6, 0.8 or 1.0 mm. The specific degree of increase in the roller gap height is selected within the above range based on the head buckle degree of the thin plate.
[0076] Step S3 also includes:
[0077] Sub-step S35, when the type of thin plate warping is head warping, lower the roller gap height by 0.3-1.0 mm.
[0078] In actual operation, for thin plates with head warping problems, lowering the roller gap height by 0.3-1.0mm can effectively eliminate the head warping problem; if the roller gap height is lowered below 0.3mm, the head warping problem may still exist, and if the roller gap height is lowered by more than 1mm, the head buckle problem may occur.
[0079] For example, when the type of warping of the thin plate is head warping, the roller gap height is reduced by 0.3, 0.6, 0.8 or 1.0 mm. The specific degree of reduction in the roller gap height is selected within the above range based on the degree of head warping of the thin plate.
[0080] Step S3 also includes:
[0081] Sub-step S36: when the head section of the thin plate becomes wavy, the roller gap height is increased by 0.5-1.5 mm, wherein the length of the head section is 0.8-1.2 m.
[0082] It should be noted that the reason why the head section of the thin plate becomes wavy is that the thin plate touches the water pressure roller, collides and rubs, causing the movement of the thin plate to be obstructed, thereby causing the head section to become wavy.
[0083] In actual operation, for thin plates with only the head section of about 1m becoming corrugated, the roller gap height should be gradually increased. For example, first increase the roller gap height by 0.5mm, and observe the shape of the thin plate after quenching. If the shaping effect is not good, increase the roller gap height by 1mm until the head section of the thin plate is flat.
[0084] For thin plates with corrugated head sections, if the roller gap height is raised to less than 0.5 mm, the adjustment effect is not obvious. If the roller gap height is raised to greater than 1.5 mm, the head warping problem may occur.
[0085] Step S3 also includes:
[0086] Sub-step S37: When the type of warping of the thin plate is tail bulging or tail warping, increase the water volume of the gap nozzle by 50m for every 10mm of unevenness. 3 / h.
[0087] The tail of the thin plate is bulging or warping, which is generally caused by insufficient cooling speed of the steel plate and uneven stress at the tail of the plate. At this time, the water volume of the gap nozzle should be increased.
[0088] In actual operation, use a two-meter ruler to measure the unevenness of the steel plate (in mm). For every 10 mm unevenness, increase the water volume of the gap nozzle by 50 mm. 3 / h.
[0089] For example, a 20 mm unevenness will increase the gap nozzle water flow by 100 m 3 / h.
[0090] In summary, the embodiment of the present application provides a method for adjusting the shape of a quenched curved plate. The steel plate is first divided into a thick plate and a thin plate according to its thickness. For the thick plate, when the type of curvature of the thick plate is a middle arch, the water ratio is increased; when the type of curvature of the thick plate is warped at both ends, the water ratio is reduced; when the type of curvature of the thick plate is a full-body boat shape, the roller speed is increased; for the thin plate, when the type of curvature of the thin plate is a middle wave, the roller speed is reduced; when the type of curvature of the thin plate is a side wave, the roller speed is increased; when the type of curvature of the thin plate is a head buckle, the roller gap height is increased; when the type of curvature of the thin plate is warped at the head, the roller gap height is reduced; when the head section of the thin plate becomes wavy, the roller gap height is increased; when the type of curvature of the thin plate is a tail bulge or tail warping, the water volume of the gap nozzle is increased. By taking corresponding adjustment measures for thick and thin plates according to different types of curvature, the quenched steel plate can reach a relatively flat state.
[0091] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for adjusting the shape of a quenching plate, applied to a quenching furnace, characterized in that: include: According to the thickness of the steel plate, the steel plate is divided into thick plate and thin plate; For thick plates, when the type of curvature is arched in the middle, increase the water ratio; when the type of curvature is warped at both ends, reduce the water ratio; when the type of curvature is boat-shaped throughout, increase the roller speed; For thin plates, when the type of curvature of the thin plates is middle waves, reduce the roller speed; when the type of curvature of the thin plates is side waves, increase the roller speed; when the type of curvature of the thin plates is head buckle, increase the roller gap height; when the type of curvature of the thin plates is head warping, reduce the roller gap height; when the head section of the thin plates becomes wavy, increase the roller gap height; when the type of curvature of the thin plates is tail bulge or tail warping, increase the water volume of the gap nozzle.
2. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the type of curvature of the thick plate is a boat shape, the step of increasing the roller speed comprises: For every 20mm upward tilt at both ends of the thick plate, increase the roller speed by 18 / H 2 m / s, where 18 is the empirical coefficient and H is the thickness of the steel plate in mm.
3. The method for adjusting the shape of a quenched curved plate according to claim 2, characterized in that: Increase the roller speed by 18 / H for every 20mm upward tilt at both ends of the thick plate. 2 After the m / s step, it also includes: For every 20mm upward tilt at both ends of the thick plate, increase the water volume of the gap nozzle by 30m 3 / h.
4. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the type of the thin plate curvature is medium wave, the step of reducing the roller speed comprises: When the type of curvature of the thin plate is medium wave, the roller speed will be reduced by 0.05m / s for every 10mm of unevenness, and the roller gap height will be reduced by 0.5mm.
5. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the type of the thin plate curvature is edge wave, the step of increasing the roller speed comprises: When the type of curvature of the thin plate is edge wave, the roller speed shall be increased by 0.05m / s for every 10mm of unevenness.
6. The method for adjusting the shape of a quenched curved plate according to claim 5, characterized in that: After the step of increasing the roller speed by 0.05 m / s for every 10 mm unevenness when the type of the thin plate curvature is edge wave, the method further includes: For every 0.05m / s increase in roller speed, increase the gap nozzle water volume by 50m 3 / h.
7. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the type of the thin plate curvature is head buckle, the step of increasing the roller gap height comprises: When the type of curvature of the thin plate is head buckle, increase the roller gap height by 0.3-1.0mm.
8. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the type of the thin plate warping is head warping, the step of reducing the roller gap height comprises: When the type of warping of the thin plate is head warping, reduce the roller gap height by 0.3-1.0mm.
9. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the head section of the thin plate becomes wavy, the step of increasing the roller gap height comprises: When the head section of the thin plate becomes corrugated, the roller gap height is increased by 0.5-1.5 mm, wherein the length of the head section is 0.8-1.2 m.
10. The method for adjusting the shape of a quenched curved plate according to claim 1, characterized in that: When the type of warping of the thin plate is tail bulging or tail warping, the step of increasing the water volume of the gap nozzle comprises: When the type of thin plate warping is tail bulging or tail warping, increase the gap nozzle water volume by 50m for every 10mm unevenness. 3 / h.