In-situ synthesis TiB2 phase reinforced Cu-Ni-Co-Al-Ti-Fe-B system wear-resistant high-temperature copper alloy and preparation method thereof
By synthesizing Cu-Ni-Co-Al-Ti-Fe-B wear-resistant high-temperature copper alloy in situ, using multi-component co-examination and solid solution of Fe, Co, and Ti elements, Ti particles were generated, and the copper alloy was solved. Insufficient strength and wear resistance at high temperatures have been achieved, significant improvement in high temperature performance and optimization of friction wear rate.
Patent Information
- Application Number
- CN202411165642.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-23
AI Technical Summary
The existing copper alloys have insufficient strength and wear resistance at high temperatures, and the preparation method leads to serious defects in material performance, especially the poor interface bond between TiB2 particles and the matrix, which limits its application.
In-situ synthesis method was used to prepare Cu-Ni-Co-Al-Ti-Fe-B wear-resistant high-temperature copper alloy, and Ti particles were generated by multi-component co-examination, combining Fe, Co and Ti elements in L12-Ni3Al phase The solid solution of the product improves the stability of high temperature, and uses Co and B elements to strengthen the alloy to achieve the in-situ generation and high temperature lubrication effect of TiB2 particles.
It significantly improves the high-temperature compression strength and elongation of copper alloys, while maintaining excellent friction coefficient and wear rate at room temperature and 900°C, which is better than similar alloys prepared by powder metallurgy, and has a simple process.
Smart Images

Figure CN119082587A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an in-situ synthesized TiB2 phase-reinforced Cu-Ni-Co-Al-Ti-Fe-B series wear-resistant high-temperature copper alloy and a preparation method thereof, and belongs to the field of high-temperature wear-resistant copper alloys. Background Art
[0002] Copper alloys have excellent electrical and thermal conductivity, good plasticity and corrosion resistance, and are widely used in rail transportation, machinery manufacturing, electronics industry and other fields. With the rapid development of industry, copper alloys are facing the service under complex working conditions such as high temperature, heavy load and high wear, and there is an urgent need to further improve the heat resistance and friction and wear resistance of the alloys. At present, there are only a handful of alloys with a softening temperature exceeding 600°C, and copper alloys have always been considered to have no suitable high temperature resistance. The use of ceramic particle reinforced powder metallurgy and in-situ synthesis of oxidized dispersed copper alloys has improved the heat resistance of copper alloys to a certain extent, but the indicators such as high temperature strength and elongation have not been comprehensively improved. The main problem is that the many defects caused by the preparation method have seriously deteriorated the material properties. For example, the copper-based composite material prepared by directly adding TiB2 particles greatly reduces the friction coefficient and wear rate, but due to the poor wettability between the matrix Cu and the reinforcing particles TiB2, poor interface bonding, low material density, complex process, and high cost, the application is limited to a certain extent. Summary of the invention
[0003] In order to improve the high temperature strength and wear resistance of copper alloys, the present invention intends to design and prepare a Cu-Ni-Co-Al-Ti-Fe-B series wear-resistant high temperature copper alloy reinforced by in-situ synthesis of TiB2 phase. Taking advantage of the multi-component characteristics, multi-scale multi-element coherent precipitation strengthening is first introduced to improve the alloy strength, elongation and high temperature stability; secondly, TiB2 particles are generated in-situ to enhance the alloy wear resistance.
[0004] The technical solution adopted by the present invention is: an in-situ synthesized TiB2 phase-enhanced Cu-Ni-Co-Al-Ti-Fe-B series wear-resistant high-temperature copper alloy, the atomic percentage composition of the copper alloy is (Cu 44 / 100 Ni 25 / 100 Co 12.5 / 100 Al 6.25 / 100 Ti 6.25 / 100 Fe 6 / 100 ) 100-x B x (x=2.5~5); the ultimate compressive strength of the copper alloy is 1440MPa~1947MPa, the elongation is 22.3%~32.8%; the room temperature friction coefficient is 0.18~0.20, and the room temperature wear rate is 1.51×10 -5 mm 3 / N·m~7.47×10 -6 mm 3 / N·m; 900℃ friction coefficient 0.42~0.38; wear rate 7.03×10 -5 mm 3 / N·m~6.27×10 -5 mm 3 / N·m.
[0005] A method for preparing a Cu-Ni-Co-Al-Ti-Fe-B series wear-resistant high-temperature copper alloy reinforced by in-situ synthesis of TiB2 phase comprises the following steps:
[0006] According to the above-mentioned composition of the alloy, high-purity metal of 4N or above is used as raw material, and a non-consumable vacuum arc melting furnace is adopted. High-purity argon gas protection is introduced to repeatedly melt the alloy raw materials prepared with the alloy components, and finally an alloy ingot with in-situ generated TiB2 particles is obtained; subsequently, the smelted alloy ingot is subjected to solid solution and aging treatment to obtain a TiB2 phase-reinforced Cu-Ni-Co-Al-Ti-Fe-B wear-resistant high-temperature copper alloy.
[0007] Preferably, the solution treatment temperature in the above steps is 1070° C., the holding time is 8 hours, and then air-cooled to room temperature.
[0008] Preferably, the aging treatment temperature in the above steps is 650° C., the holding time is 4 hours, and then the furnace is cooled to room temperature.
[0009] The alloy was subjected to compression test using a universal testing machine, and the friction performance of the alloy was tested using a friction and wear testing machine.
[0010] The beneficial effects of the present invention are:
[0011] Multi-component coherent precipitation strengthening is an effective way to improve the high-temperature properties of copper alloys. Multi-components can synthesize high-temperature lubricating phase TiB2 in situ and control reasonable microstructure morphology, specifically:
[0012] (1) The high temperature stability of the precipitated phase is improved by solid solution of alloying elements such as Fe, Co and Ti in the basic strengthening phase L12-Ni3Al phase, and its high temperature dissolution is delayed. (2) The strength and high temperature stability of the matrix are improved by solid solution of alloying elements such as Fe, Co and Ti in the copper matrix. (3) The elongation of the alloy is improved by the effect of elements that reduce stacking fault energy (such as Co) and grain boundary strengthening elements (such as B). (4) Ti and B elements generate TiB2 particles in situ, which play a role of high temperature lubrication while strengthening. Based on this, the compressive strength and elongation of the alloy obtained by the present invention are significantly better than those of similar alloys prepared by powder metallurgy, and can maintain outstanding friction coefficient and wear rate at room temperature and 900°C. At present, there is no report on copper alloys and copper-based composite materials that can serve at 900°C. This alloy is prepared by vacuum arc melting, which is a simple method. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Cu after aging treatment 42.9 Ni 24.375 Co 12.1875 Al 6.09375 Ti 6.09375 Fe 5.85 B 2.5 Room temperature compressive engineering stress-strain curves of (at.%) alloy.
[0014] Figure 2 Cu after aging treatment 42.9 Ni 24.375 Co 12.1875 Al 6.09375 Ti 6.09375 Fe 5.85 B 2.5 Friction coefficient and wear scar width / depth diagrams of the alloy at room temperature and 900 °C (at.%) (inset).
[0015] Figure 3 Cu after aging treatment 41.8 Ni 23.75 Co 11.875 Al 5.9375 Ti 5.9375 Fe 5.7 Room temperature compressive engineering stress-strain curves of B5(at.%) alloy.
[0016] Figure 4 Cu after aging treatment 41.8 Ni 23.75 Co 11.875 Al 5.9375 Ti 5.9375 Fe 5.7 Friction coefficient and wear scar width / depth plots of B5 (at.%) alloy at room temperature and 900 °C (inset). DETAILED DESCRIPTION
[0017] The specific embodiments of the present invention are described in detail below in conjunction with the technical solutions.
[0018] Example 1: Cu 42.9 Ni 24.375 Co 12.1875 Al 6.09375 Ti 6.09375 Fe 5.85 B 2.5 (at.%) Alloy
[0019] Step 1: Alloy preparation
[0020] 1. According to the alloy composition Cu 42.9 Ni 24.375 Co 12.1875 Al 6.09375 Ti 6.09375 Fe 5.85 B 2.5 (at.%), using 5N purity Cu and Al, 4N purity Ni, Co, Ti, Fe, B raw materials to prepare the alloy; using a non-consumable vacuum arc melting furnace, passing high-purity argon gas protection, repeatedly melting the prepared alloy raw materials for 5 times, and finally obtaining an alloy ingot with in-situ generated TiB2 particles;
[0021] 2. Compression specimen preparation: The alloy was solution treated at 1070°C for 8 h, air-cooled to room temperature, and then kept at 650°C for 4 h, and furnace-cooled to room temperature for aging treatment.
[0022] 3. Preparation of friction and wear samples: The alloy was solution treated at 1070 °C for 8 h, air-cooled to room temperature, and then kept at 650 °C for 4 h and furnace-cooled to room temperature for aging treatment.
[0023] Step 2: Performance Characterization
[0024] 1. The mechanical properties of the alloy samples were analyzed using a UTM5504 electronic universal testing machine. The room temperature compression test was conducted according to the national standard GB / T 7314-2017 for room temperature compression tests of metal materials, with a nominal strain rate of 0.005 min -1 According to the obtained stress-strain curve, the mechanical properties of the material are obtained: the ultimate compressive strength is 1440MP, the elongation is 22.3%, such as Figure 1 shown.
[0025] 2. The friction and wear properties of the alloy were tested using a UMT-3 friction and wear tester. The friction and wear test conditions are shown in Table 1. The room temperature friction coefficient is 0.18, and the room temperature wear rate is 1.51×10-5 mm 3 / N·m; friction coefficient at 900℃ is 0.42; wear rate is 7.03×10 -5 mm 3 / N·m, such as Figure 2 shown.
[0026] Table 1 Alloy friction and wear test conditions
[0027] Test temperature ℃ Friction pair material / diameter Contact stress MPa Friction rate mm / s Friction time min 25 <![CDATA[Al2O3 / 6mm]]> 262 1 10 900 <![CDATA[Al2O3 / 6mm]]> 262 1 10
[0028] Example 2: Cu 41.8 Ni 23.75 Co 11.875 Al 5.9375 Ti 5.9375 Fe 5.7 B5(at.%) alloy
[0029] Step 1: Alloy preparation
[0030] 1. According to the alloy composition Cu 41.8 Ni 23.75 Co 11.875 Al 5.9375 Ti 5.9375 Fe 5.7 B5 (at.%), using 5N purity Cu and Al, 4N purity Ni, Co, Ti, Fe, B raw materials to prepare the alloy; using a non-consumable vacuum arc melting furnace, passing high-purity argon gas protection, repeatedly smelting the prepared alloy raw materials for 5 times, and finally obtaining an alloy ingot with in-situ generated TiB2 particles;
[0031] 2. Compression specimen preparation: The alloy was solution treated at 1070°C for 8 h, air-cooled to room temperature, and then kept at 650°C for 4 h, and furnace-cooled to room temperature for aging treatment.
[0032] 3. Preparation of friction and wear samples: The alloy was solution treated at 1070 °C for 8 h, air-cooled to room temperature, and then kept at 650 °C for 4 h and furnace-cooled to room temperature for aging treatment.
[0033] Step 2: Performance Characterization
[0034] 1. The mechanical properties of the alloy samples were analyzed using a UTM5504 electronic universal testing machine. The room temperature compression test was conducted according to the national standard GB / T 7314-2017 for room temperature compression tests of metal materials, with a nominal strain rate of 0.005 min -1 According to the obtained stress-strain curve, the mechanical properties of the material are obtained: the ultimate compressive strength is 1947MP, the elongation is 32.8%, such as Figure 3 shown.
[0035] The friction and wear properties of the alloy were tested using a UMT-3 friction and wear tester. The friction and wear test conditions are shown in Table 1. The room temperature friction coefficient is 0.18, and the room temperature wear rate is 7.47×10 -6 mm 3 / N·m; friction coefficient at 900℃ is 0.38; wear rate is 6.27×10 -5 mm 3 / N·m, such as Figure 4 shown.
Claims
1. An in-situ synthesized TiB2 phase-enhanced Cu-Ni-Co-Al-Ti-Fe-B wear-resistant high-temperature copper alloy, characterized in that: The atomic percentage composition of the copper alloy is (Cu 44 / 100 Ni 25 / 100 Co 12.5 / 100 Al 6.25 / 100 Ti 6.25 / 100 Fe 6 / 100 ) 100-x B x , where x = 2.5~5; The ultimate compressive strength of the copper alloy is 1440MPa~1947MPa, the elongation is 22.3%~32.8%, the room temperature friction coefficient is 0.18~0.20, and the room temperature wear rate is 1.51×10 -5 mm 3 / N·m~7.47×10 -6 mm 3 / N·m; the friction coefficient at 900℃ is 0.42~0.38, and the wear rate is 7.03×10 -5 mm 3 / N·m~6.27×10 -5 mm 3 / N·m.
2. The method for preparing a wear-resistant high-temperature copper alloy of the Cu-Ni-Co-Al-Ti-Fe-B series reinforced by in-situ synthesis of TiB2 phase according to claim 1, characterized in that: The following steps are involved: Using high-purity metal of 4N or above as raw material, adopting a non-consumable vacuum arc melting furnace, passing high-purity argon gas protection, melting the alloy raw material prepared according to the alloy composition of claim 1, and finally obtaining an alloy ingot with in-situ generated TiB2 particles; Subsequently, the smelted alloy ingot is subjected to solid solution and aging treatment to obtain a TiB2 phase-reinforced Cu-Ni-Co-Al-Ti-Fe-B wear-resistant high-temperature copper alloy.
3. The preparation method according to claim 2, characterized in that: The solution treatment temperature is 1070℃, the holding time is 8h, and then air-cooled to room temperature.
4. The preparation method according to claim 2, characterized in that: The aging treatment temperature is 650°C, the holding time is 4h, and then the furnace is cooled to room temperature.
Citation Information
Patent Citations
Cu-Al-Ti-Fe-Ni system copper alloy
CN104928524A
High-strength heat-resistant conductive copper alloy pipe and preparation method thereof
CN115198133A
Multi-scale multiphase coherent precipitation strengthened Cu-Ni-Al-Co-Cr-Ti high-temperature-resistant copper alloy and preparation method thereof
CN116555625A
TiB2 / Cu-B composite material for current-carrying frictional wear and preparation method of TiB2 / Cu-B composite material
CN118516586A
Copper alloy and producing method therefor
CN1540012A