Low-yield-strength deep-drawing zinc plating material and preparation method thereof
By adjusting the hot-pressing coil and galvanizing process parameters, the yield strength of DX53D hot-dip galvanized plate is solved, and the problem of excessive yield strength in the existing technology is improved, achieving cost-effectiveness.
Patent Information
- Application Number
- CN202411194426.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, the yield strength of DX53D hot-dip galvanized products is prone to exceed 170Mpa, resulting in stamping cracking, and reducing the yield strength requires substantial improvement of raw materials or processes, resulting in high costs.
By adjusting the preparation process, galvanizing process and pulling process of the hot-pressing coil, the element content and process parameters in the hot-pressing coil are controlled, such as carbon ≤0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, Phosphorus: 0.012%, titanium ≤0.04%, final rolling temperature is 730-735℃, annealing temperature is 840-845℃, galvanizing speed is 70-80m/min, photo-integration pressure is 120-128 tons, stretching machine extension The rate is 0.8-1% to reduce the yield strength of the galvanized sheet.
While ensuring surface quality, the yield strength of the galvanized plate is reduced to below 170Mpa, meets performance requirements, and achieves results through small adjustments, saving the cost of purchasing new raw materials or equipment.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of galvanized steel strips, and in particular to a low-yield strength deep-drawn galvanized material and a preparation method thereof. Background Art
[0002] Low-yield DX53D hot-dip galvanized products are widely used in the field of home appliance substrates. In actual use, once the yield strength of DX53D hot-dip galvanized products exceeds 170Mpa, it is easy to cause abnormal stamping cracking during the stamping process. Therefore, the yield strength of qualified DX53D hot-dip galvanized products must be controlled below 170Mpa.
[0003] In the prior art: the carbon content in the hot-pressed coil is 0.001-0.007%; during the preparation of the hot-pressed coil, the final rolling temperature is 730-735°C; the annealing temperature is 840-845°C; the skin-passing pressure is 120-128 tons; the elongation of the tension leveler is 0.8-1%; the yield strength of the obtained low-yield DX53D hot-dip galvanized product needs to be controlled above 170Mpa.
[0004] In order to reduce the yield strength, it is usually necessary to make significant improvements in raw materials or processes, which incurs the cost of purchasing new raw materials, new equipment or opening a new production line.
[0005] Based on this, the present invention designs a low yield strength deep drawing galvanized material and a preparation method thereof to solve the above problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a low yield strength deep-drawn galvanized material and a preparation method thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A low yield strength deep drawing galvanized material, characterized by comprising a hot pressed coil and a galvanized layer outside the hot pressed coil;
[0009] In the hot pressed coil, carbon ≤0.002%, silicon: 0.008-0.012%, manganese: 0.08-0.12%, sulfur: 0.008-0.012%, phosphorus: 0.008-0.012%, titanium ≤0.04%; the balance is iron.
[0010] Furthermore, in the hot pressed coil, carbon ≤0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤0.04%; the balance is iron.
[0011] A method for preparing a low yield strength deep-drawn galvanized DX53D material comprises the following steps:
[0012] Step 1: preparing hot pressed coil;
[0013] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0014] Step 2: After the hot rolled coil is cold rolled, it is galvanized and annealed. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0015] Step 3: Obtain low yield strength deep-drawn galvanized material through skin straightening and straightening.
[0016] Furthermore, the yield strength of the low yield strength deep-drawn galvanized material obtained in step three is below 170 MPa.
[0017] Furthermore, in step 1, during the preparation of the hot pressed coil, the final rolling temperature is 730-735°C.
[0018] Furthermore, in step 2, the annealing temperature is 840-845°C.
[0019] Furthermore, in step 2, the galvanizing speed is 70-80 m / min.
[0020] Furthermore, in step three, during the finishing process, the finishing pressure is 120-128 tons.
[0021] Furthermore, in step three, during the straightening process, the elongation of the straightening machine is 0.8-1%.
[0022] Compared with the prior art, the present invention has the following beneficial effects: 1. By adjusting the preparation process of the hot-pressed coil, the galvanizing process, the galvanizing finishing process and the straightening process, the yield strength of the galvanized sheet is reduced to below 170 MPa while ensuring stable surface quality, thereby meeting the performance requirements of the galvanized sheet.
[0023] 2. The process steps of the present invention are simple, and only minor adjustments can be made on the basis of the existing technology. There is no need to purchase additional instruments or raw materials. Significant effects can be obtained through relatively small process adjustment costs, so that the yield strength is significantly reduced, saving the cost of purchasing new raw materials, new equipment or opening new production lines. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1: This embodiment provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0026] Step 1: preparing hot pressed coil;
[0027] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.012%, manganese: 0.12%, sulfur: 0.012%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0028] During the preparation of the hot pressed coil, the final rolling temperature is 735°C;
[0029] Step 2: After the hot rolled coil is cold rolled, it is galvanized and annealed at 845°C. The annealed strip (the strip is released from the hot pressed coil) passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0030] The galvanizing speed is 80m / min;
[0031] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0032] During the finishing process, the finishing pressure is 128 tons;
[0033] During the straightening process, the elongation of the straightening machine is 1%.
[0034] Embodiment 2: This embodiment provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0035] Step 1: preparing hot pressed coil;
[0036] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.008%, manganese: 0.08%, sulfur: 0.008%, phosphorus: 0.008%, titanium ≤ 0.04%; the balance is iron;
[0037] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0038] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0039] The galvanizing speed is 70m / min;
[0040] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0041] During the finishing process, the finishing pressure is 120 tons;
[0042] During the straightening process, the elongation of the straightening machine is 0.8%.
[0043] Embodiment 3: This embodiment provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0044] Step 1: preparing hot pressed coil;
[0045] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0046] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0047] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0048] The galvanizing speed is 80m / min;
[0049] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0050] During the finishing process, the finishing pressure is 120 tons;
[0051] During the straightening process, the elongation of the straightening machine is 0.9%.
[0052] Embodiment 4: This embodiment provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0053] Step 1: preparing hot pressed coil;
[0054] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.008%, manganese: 0.08%, sulfur: 0.008%, phosphorus: 0.008%, titanium ≤ 0.04%; the balance is iron;
[0055] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0056] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0057] The galvanizing speed is 80m / min;
[0058] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0059] During the finishing process, the finishing pressure is 120 tons;
[0060] During the straightening process, the elongation of the straightening machine is 0.9%.
[0061] Embodiment 5: This embodiment provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0062] Step 1: preparing hot pressed coil;
[0063] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.012%, manganese: 0.12%, sulfur: 0.012%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0064] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0065] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0066] The galvanizing speed is 80m / min;
[0067] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0068] During the finishing process, the finishing pressure is 120 tons;
[0069] During the straightening process, the elongation of the straightening machine is 0.9%.
[0070] Comparative Example 1: This comparative example provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0071] Step 1: preparing hot pressed coil;
[0072] In the hot pressed coil, carbon ≤ 0.001%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0073] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0074] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0075] The galvanizing speed is 80m / min;
[0076] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0077] During the finishing process, the finishing pressure is 120 tons;
[0078] During the straightening process, the elongation of the straightening machine is 0.9%.
[0079] Comparative Example 2: This comparative example provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0080] Step 1: preparing hot pressed coil;
[0081] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0082] During the preparation of the hot pressed coil, the final rolling temperature is 720°C;
[0083] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0084] The galvanizing speed is 80m / min;
[0085] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0086] During the finishing process, the finishing pressure is 120 tons;
[0087] During the straightening process, the elongation of the straightening machine is 0.9%.
[0088] Comparative Example 3: This comparative example provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0089] Step 1: preparing hot pressed coil;
[0090] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0091] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0092] Step 2: The hot pressed coil releases the strip, which is annealed at 810°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0093] The galvanizing speed is 80m / min;
[0094] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0095] During the finishing process, the finishing pressure is 120 tons;
[0096] During the straightening process, the elongation of the straightening machine is 0.9%.
[0097] Comparative Example 4: This comparative example provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0098] Step 1: preparing hot pressed coil;
[0099] In the hot pressed coil, carbon ≤ 0.007%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0100] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0101] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0102] The galvanizing speed is 80m / min;
[0103] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0104] During the finishing process, the finishing pressure is 120 tons;
[0105] During the straightening process, the elongation of the straightening machine is 0.9%.
[0106] Comparative Example 5: This comparative example provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0107] Step 1: preparing hot pressed coil;
[0108] In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron;
[0109] During the preparation of the hot pressed coil, the final rolling temperature is 730°C;
[0110] Step 2: The hot pressed coil releases the strip, which is annealed at 840°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0111] The galvanizing speed is 80m / min;
[0112] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0113] During the finishing process, the finishing pressure is 170 tons;
[0114] During the straightening process, the elongation of the straightening machine is 0.9%.
[0115] Comparison Example
[0116] This comparative example provides a method for preparing a low yield strength deep-drawn galvanized DX53D material, comprising the following steps:
[0117] Step 1: preparing hot pressed coil;
[0118] The hot pressed coil contains 0.001-0.007% carbon, 0.01% silicon, 0.10% manganese, 0.010% sulfur, 0.012% phosphorus, and ≤0.04% titanium; the remainder is iron;
[0119] During the preparation of the hot pressed coil, the final rolling temperature is 720°C;
[0120] Step 2: The hot pressed coil releases the strip, which is annealed at 810°C. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing.
[0121] Step 3: Obtain low yield strength deep-drawn galvanized DX53D material through skin-passing and straightening;
[0122] During the finishing process, the finishing pressure is 170 tons;
[0123] During the straightening process, the elongation of the straightening machine is 0.5%.
[0124] The yield strength of the galvanized DX53D material obtained in Example 3 and Comparative Examples 1-5 or the control example was tested according to GB / T 28905-2022 standard, and the results are as follows:
[0125] Table 1
[0126] project Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Example 3 Carbon content 0.001% 0.002% 0.002% 0.007% 0.002% 0.002% Finishing rolling temperature 730℃ 720℃ 730℃ 730℃ 730℃ 730℃ Annealing temperature 840℃ 840℃ 810℃ 840℃ 840℃ 840℃ Finishing pressure 120 tons 120 tons 120 tons 120 tons 170 tons 120 tons Elongation of tension leveler 0.9% 0.9% 0.9% 0.9% 1.5% 0.9% Yield Strength 168Mpa 175Mpa 180Mpa 180Mpa 165Mpa ≤170Mpa
[0127] Table 2
[0128] project Comparison Example Example 3 Carbon content 0.001% 0.002% Finishing rolling temperature 720℃ 730℃ Annealing temperature 810℃ 840℃ Finishing pressure 170 tons 120 tons Elongation of tension leveler 1.5% 0.9% Yield Strength 178Mpa ≤170Mpa
[0129] Result analysis: From Table 1, it can be concluded that the yield strength of the products prepared in Comparative Examples 1 and 5 is below 170 MPa. However, it is difficult to control the carbon content at 0.001% in practice, and the yield strength of the galvanized material does not change much with the carbon content of 0.002%. In Comparative Example 5, the skin-passing pressure is increased to 170 tons, and the yield strength of the galvanized material does not change much with the skin-passing pressure of 120 tons. Therefore, considering the cost and benefit comprehensively, the carbon content of 0.002%, the final rolling temperature of 730°C, the annealing temperature of 840°C, the skin-passing pressure of 120 tons, and the elongation of the straightening machine of 0.9% are the best process (i.e., Example 3);
[0130] The present invention reduces the yield strength of the galvanized sheet to below 170 MPa while ensuring stable surface quality by adjusting the preparation process of the hot-pressed coil, the galvanizing process, the galvanizing skin-finishing process and the straightening process, thereby meeting the performance requirements of the galvanized sheet.
[0131] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low yield strength deep drawing galvanized material, characterized in that: Including hot pressed coil and galvanized layer outside the hot pressed coil; In the hot pressed coil, carbon ≤0.002%, silicon: 0.008-0.012%, manganese: 0.08-0.12%, sulfur: 0.008-0.012%, phosphorus: 0.008-0.012%, titanium ≤0.04%; the balance is iron.
2. The low yield strength deep-drawn galvanized material according to claim 1, characterized in that: In the hot pressed coil, carbon is ≤0.002%, silicon is 0.01%, manganese is 0.10%, sulfur is 0.010%, phosphorus is 0.012%, titanium is ≤0.04%; and the balance is iron.
3. A method for preparing a low yield strength deep-drawn galvanized material as claimed in claim 1 or 2, characterized in that: The following steps are involved: Step 1: preparing hot pressed coil; In the hot pressed coil, carbon ≤ 0.002%, silicon: 0.01%, manganese: 0.10%, sulfur: 0.010%, phosphorus: 0.012%, titanium ≤ 0.04%; the balance is iron; Step 2: After the hot rolled coil is cold rolled, it is galvanized and annealed. The annealed strip passes through the zinc pot and is coated with zinc liquid. The excess zinc liquid on the surface of the strip is blown off by an air knife to complete the galvanizing. Step 3: Obtain low yield strength deep-drawn galvanized material through skin straightening and straightening.
4. The method for preparing a low yield strength deep-drawn galvanized material according to claim 3, characterized in that: In step 1, during the preparation of the hot pressed coil, the final rolling temperature is 730-735°C.
5. The method for preparing a low yield strength deep-drawn galvanized material according to claim 4, characterized in that: In step 2, the annealing temperature is 840-845°C.
6. The method for preparing a low yield strength deep-drawn galvanized material according to claim 5, characterized in that: In step 2, the galvanizing speed is 70-80m / min.
7. The method for preparing a low yield strength deep-drawn galvanized material according to claim 6, characterized in that: In step 3, during the finishing process, the finishing pressure is 120-128 tons.
8. The method for preparing a low yield strength deep-drawn galvanized material according to claim 7, characterized in that: In step 3, during the straightening process, the elongation of the straightening machine is 0.8-1%.