PLC defect elimination method and aluminum alloy plate production method

By keeping the temperature not lower than 25°C after quenching and cooling of the aluminum alloy sheet and performing pre-stretching treatment, the problem of PLC defects is solved, production efficiency and equipment utilization are improved, and the surface quality of the sheet is ensured.

CN119082630APending Publication Date: 2024-12-06SHANDONG NANSHAN ALUMINUM +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411201878.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing aluminum alloy sheets are prone to surface slip line defects (PLC defects) during pre-stretching treatment, resulting in uneven deformation and reduced forming capacity of the sheet, and long-term natural aging reduces production efficiency and equipment usage.

Method used

By keeping the temperature not lower than 25°C after quenching and cooling of the aluminum alloy, and performing pre-stretching treatment on this basis, the interval between quenching and pre-stretching treatment is shortened, and spraying of the hard quenching section and the soft quenching section is adopted. The cooling water is cooled down, and the temperature of the soft quenching section is controlled to be 30℃.

Benefits of technology

It significantly improves the pinning strength and pinning chance of movable dislocations by solute atoms, increases the critical tensile deformation of PLC defects, avoids the occurrence of PLC defects after pre-stretching, and improves production efficiency and equipment use. The surface quality of the board is guaranteed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082630A_ABST
    Figure CN119082630A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy production, and provides a PLC defect elimination method which comprises the following steps: carrying out solution treatment on an aluminum alloy part, and carrying out heat preservation for a preset duration; quenching and cooling the aluminum alloy part; the temperature of the quenched and cooled aluminum alloy part is controlled to be not lower than 25 DEG C; and after quenching cooling, the aluminum alloy part is placed for a preset time length, and pre-stretching treatment is conducted on the aluminum alloy part. Therefore, the temperature of the aluminum alloy part after quenching and cooling is controlled; the activity of solute atoms is kept, the pinning strength and the pinning probability of the solute atoms to movable dislocation are improved, the difficulty of the solute atoms getting rid of pinning is increased, and the PLC defect after prestretching is avoided. According to the method, the interval time between quenching cooling and pre-stretching treatment is remarkably shortened, the yield strength of the aluminum alloy part is prevented from being increased, and the requirement for pre-stretching equipment is lowered. And the production efficiency is improved, and the qualified rate of the surface quality of products is guaranteed. The invention further provides a production method of the aluminum alloy plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy production, and in particular relates to a PLC defect elimination method and an aluminum alloy plate production method. Background Art

[0002] After the solution treatment, the heat-treatable strengthened aluminum alloy plate is subjected to a pre-stretching treatment to cause permanent plastic deformation (the deformation is usually 1.5-3.0%) in the rolling direction of the plate to reduce the residual stress.

[0003] However, the sheet is prone to surface slip line defects (Portevin-Le Chatelier effect, referred to as PLC defects) during the pre-stretching process, which affects the surface quality defects of the sheet, causes obvious differences in the organization of different areas of the sheet, aggravates the uneven deformation of the sheet, reduces the forming ability, and even causes fracture failure.

[0004] At the microstructural level, the movable dislocations in the aluminum alloy sheet are blocked by obstacles such as forest dislocations during their movement. Solute atoms are concentrated toward the blocked movable dislocations by diffusion, forming solute atom gas clusters. The atomic gas clusters will exert additional pinning on the dislocations. During pre-stretching, the sheet is subjected to external forces, causing the movable dislocations to restart on a large scale in a thermally activated manner, resulting in depinning. The repeated pinning and depinning between solute atoms and movable dislocations is manifested as PLC defects in the macroscopic morphology.

[0005] In order to avoid PLC defects, the existing process scheme is usually: the plate is subjected to a long period of natural aging after solution treatment. During the natural aging process, the concentration of solid solution atoms in the alloy decreases, and GP zones are continuously formed. The movement of mobile dislocations is hindered, making them more easily pinned by solute atoms. At the same time, during this period, more atoms are concentrated toward the dislocations, which increases the pinning strength and makes it more difficult for mobile dislocations to escape the pinning of solid solution atoms. This increases the critical tensile deformation for the occurrence of PLC defects. When this deformation exceeds the permanent deformation of the pre-stretching of the plate (usually 1.5-3.0%), no PLC defects will occur on the surface of the plate.

[0006] The natural aging time varies according to the thickness of the plate, such as 6-8h for thick plates and 48-72h for thin plates. Long-term natural aging also reduces production efficiency and equipment utilization.

[0007] However, long-term natural aging also increases the yield strength of the plate, increases the deformation resistance, and increases the requirements for equipment capabilities. For thicker plates, their deformation resistance even exceeds the equipment capacity, resulting in the inability to complete the pre-stretching process. At the same time, long-term natural aging also leads to enhanced precipitation effects, reducing the consistency of the plate's overall performance and stress corrosion resistance.

[0008] In summary, the prior art obviously has inconveniences and defects in practical use, so it is necessary to improve it. Summary of the invention

[0009] In view of the above defects, the present invention mainly provides a PLC defect elimination method to solve the technical problem that after the aluminum alloy solid solution treatment, long-term natural aging leads to an increase in the yield strength of the plate and increases the difficulty of pre-stretching treatment.

[0010] In order to solve the above problems, the present invention provides a PLC defect elimination method, comprising the following steps:

[0011] S1, the aluminum alloy parts are solution treated and kept warm for a predetermined period of time:

[0012] S2, the aluminum alloy parts are quenched and cooled;

[0013] Control the temperature of aluminum alloy parts after quenching and cooling to no less than 25℃;

[0014] S3, after quenching and cooling, the aluminum alloy part is placed for a predetermined period of time to perform pre-stretching treatment.

[0015] According to the PLC defect elimination method of the present invention, during the placement process and during the pre-stretching process, the temperature of the aluminum alloy part is not lower than 25°C.

[0016] According to the PLC defect elimination method of the present invention, the aluminum alloy part is placed for no more than 24 hours after quenching and cooling.

[0017] According to the PLC defect elimination method of the present invention, the aluminum alloy part is placed for 20-30 minutes after quenching and cooling.

[0018] According to the PLC defect elimination method of the present invention, the quenching cooling process includes:

[0019] Hardening stage: The aluminum alloy parts are cooled rapidly, and a supersaturated solid solution structure is formed inside;

[0020] Soft quenching stage: The temperature of the aluminum alloy part is further reduced, and its temperature is not lower than 25℃.

[0021] According to the PLC defect elimination method of the present invention, the aluminum alloy part is cooled by spraying cooling water on it in both the hard quenching section and the soft quenching section; in the soft quenching section, the temperature of the sprayed cooling water is not lower than 25°C.

[0022] According to the PLC defect elimination method of the present invention, the spray cooling water used in the soft quenching section is obtained by mixing the water sprayed in the hard quenching section with cold water in a predetermined proportion; the temperature of the spray cooling water in the soft quenching section is controlled at 30°C.

[0023] A method for producing an aluminum alloy sheet comprises the following steps:

[0024] Z1, casting heat-treatable strengthened aluminum alloy flat ingot;

[0025] Z2, performing homogenization heat treatment on the aluminum alloy slab;

[0026] Z3, heating the aluminum alloy flat ingot to 420° C., taking it out of the furnace and rolling it into a plate;

[0027] Z4, using the PLC defect elimination method to process the plate.

[0028] According to the aluminum alloy sheet production method of the present invention, the aluminum alloy slab is subjected to homogenization heat treatment using a three-stage homogenization system, including:

[0029] Heat to 400-405°C at a heating rate of ≥40°C / h and keep warm for 3h;

[0030] Heat to 445-460℃ at a heating rate of ≥40℃ / h and keep warm for 10-24h;

[0031] Heat to 485-496°C at a heating rate of ≥30°C / h and keep warm for 8-24h.

[0032] According to the aluminum alloy sheet production method of the present invention, the material of the aluminum alloy sheet is: 2xxx, 6xxx or 7xxx series aluminum alloy.

[0033] In summary, the PLC defect elimination method of the present invention controls the temperature of the aluminum alloy parts after quenching and cooling to not less than 25°C; maintains the activity of the solute atoms, improves the pinning strength and pinning probability of the solute atoms on the movable dislocations, and makes it more difficult for the solute atoms to get rid of the pinning, thereby increasing the critical tensile deformation for the occurrence of PLC defects. PLC defects are avoided after pre-stretching. Compared with the long-term natural aging of the existing scheme, the present invention significantly shortens the interval time between quenching and pre-stretching treatment, improves the effect of pre-stretching to eliminate residual stress, and reduces the requirements for pre-stretching equipment. Improves production efficiency and ensures the qualified rate of product surface quality. The present invention also provides a method for producing aluminum alloy plates, which are treated by the PLC defect elimination method to improve the surface quality of the plates. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a surface morphology diagram of a comparative example of the present invention;

[0035] Figure 2 is a surface topography diagram of an embodiment of the present invention;

[0036] Figure 3is a tissue morphology diagram of a comparative example of the present invention;

[0037] Figure 4 is a tissue morphology diagram of an embodiment of the present invention;

[0038] in:

[0039] Figure 1 and Figure 2 The surface morphology of the surface is obtained by topological morphology analyzer.

[0040] Figure 3 and Figure 4 The organizational morphology was obtained by transmission electron microscopy (TEM). DETAILED DESCRIPTION

[0041] See also Figure 1 The present invention provides a PLC defect elimination method, comprising:

[0042] S1, the aluminum alloy parts are solution treated and kept warm for a predetermined period of time:

[0043] S2, the aluminum alloy parts are quenched and cooled;

[0044] Control the temperature of aluminum alloy parts after quenching and cooling to no less than 25℃;

[0045] S3, after quenching and cooling, the aluminum alloy part is placed for a predetermined period of time to perform pre-stretching treatment.

[0046] The material of the aluminum alloy part of the present invention is: heat-treatable and strengthened aluminum alloy. The aluminum alloy part is obtained by thermal processing, such as an aluminum alloy sheet obtained by hot rolling, or an aluminum alloy profile obtained by extrusion molding.

[0047] The solution treatment process of aluminum alloy parts can be adaptively set according to the actual shape, size, etc. using common knowledge.

[0048] After quenching and cooling, the temperature of the aluminum alloy part of the present invention is not less than 25°C. At this temperature, the solute atoms of the aluminum alloy part are highly active and move relatively quickly, which increases the pinning strength and pinning probability of the solute atoms on the movable dislocations, making it more difficult for the solute atoms to get rid of the pinning, thereby increasing the critical tensile deformation for the occurrence of PLC defects. The critical tensile deformation is much larger than the 1.5-3.0% deformation specified by the pre-stretching treatment.

[0049] The inventor has conducted multiple tests to verify that the aluminum alloy parts have a deformation of 8% during pre-stretching, but no PLC defects appear on the surface. It is proved that the critical tensile deformation of the aluminum alloy parts treated by the steps of the PLC defect elimination method of the present invention is greater than 8%. The guarantee factor of the pre-stretching process is significantly improved, so that the aluminum alloy parts can meet the requirements of various pre-stretching amounts.

[0050] Compared with the existing process scheme, the present invention can perform pre-stretching treatment without long-term natural aging, and after pre-stretching, no PLC defects appear on the surface of the aluminum alloy part.

[0051] As an implementation method, during the placement process and the pre-stretching process, the temperature of the aluminum alloy part is not less than 25° C. This allows the aluminum alloy part to have a larger critical tensile deformation and avoids PLC defects after pre-stretching.

[0052] Optionally, those skilled in the art may control the temperature of the aluminum alloy parts by controlling the ambient temperature of the production workshop.

[0053] As an implementation mode, the aluminum alloy part of the present invention can be pre-stretched after being quenched and cooled for a short time, so as to avoid long-term storage, which will increase the precipitation phase and increase the deformation resistance.

[0054] The aluminum alloy part of the present invention is placed for no more than 24 hours after quenching and cooling, and those skilled in the art can make adaptive regulations based on actual production conditions and production rhythm.

[0055] The existing technology uses long-term natural aging, which makes it difficult for the pre-stretching treatment to effectively eliminate the residual stress.

[0056] The placement time of the present invention can be significantly shortened, effectively ensuring the effect of pre-stretching treatment on eliminating residual stress.

[0057] The placement time of the present invention is not limited, and a proper time can be set according to the production rhythm.

[0058] Preferably, the aluminum alloy part of the present invention is placed for no more than 30 minutes after quenching and cooling, such as 20-30 minutes;

[0059] Preferably, the aluminum alloy part of the present invention is placed for 10 minutes, 15 minutes or 20 minutes after quenching and cooling;

[0060] After that, pre-stretching treatment is performed. The surface quality of the aluminum alloy parts after pre-stretching is guaranteed, and the production efficiency is improved. The present invention significantly shortens the interval time between quenching cooling and pre-stretching treatment, avoids the increase of the yield strength of the aluminum alloy parts, reduces the requirements for pre-stretching equipment, and improves the process assurance of the pre-stretching operation.

[0061] As an embodiment, the quenching cooling process includes:

[0062] Hardening stage: The aluminum alloy parts are cooled rapidly, and the internal structure forms a supersaturated solid solution;

[0063] Soft quenching stage: the temperature of the aluminum alloy parts is further reduced and the temperature is not lower than 25°C;

[0064] Optionally, the present invention cools the aluminum alloy part by spraying cooling water in both the hard quenching stage and the soft quenching stage; in the soft quenching stage, the temperature of the sprayed cooling water is not less than 25° C., preferably 30° C., so that the temperature of the aluminum alloy part is not less than 25° C. during the placement process after quenching and cooling.

[0065] Furthermore, the spray cooling water used in the soft quenching section of the present invention is obtained by mixing the water sprayed in the hard quenching section with cold water in a predetermined ratio; the temperature of the water sprayed in the hard quenching section is relatively high, and the temperature of the spray cooling water in the soft quenching section can be controlled at 30°C by mixing cold water in proportion. By detecting the temperatures of the water and cold water sprayed in the hard quenching section and determining the mixing ratio, the water temperature of the spray cooling water in the soft quenching section can be accurately controlled, thereby controlling the temperature of the aluminum alloy part after quenching and cooling within a predetermined range, such as 30±1°C.

[0066] The present invention also provides a method for producing an aluminum alloy sheet, comprising the following steps:

[0067] Z1, casting heat-treatable strengthened aluminum alloy flat ingot;

[0068] Z2, performing homogenization heat treatment on the aluminum alloy slab to eliminate residual stress and reduce chemical composition non-uniformity;

[0069] Preferably, the aluminum alloy slab of the present invention is subjected to homogenization heat treatment using a three-stage homogenization system, comprising:

[0070] Heat to 400-405°C at a heating rate of ≥40°C / h and keep warm for 3h;

[0071] Heat to 445-460℃ at a heating rate of ≥40℃ / h and keep warm for 10-24h;

[0072] Heat to 485-496°C at a heating rate of ≥30°C / h and keep warm for 8-24h.

[0073] Z3, heating the aluminum alloy flat ingot to 420° C., taking it out of the furnace and rolling it into a plate;

[0074] Optionally, the rolling process of the present invention is: multiple-pass reciprocating rolling.

[0075] Z4, using the PLC defect elimination method to process the plate;

[0076] Z5, ultrasonic nondestructive testing of the plate;

[0077] Z6, inspect the board length, and pack and ship the qualified boards;

[0078] The material of the heat-treatable and strengthened aluminum alloy plate of the present invention is: 2xxx, 6xxx or 7xxx series aluminum alloy.

[0079] The present invention uses a heat-treatable and strengthened aluminum alloy, the composition of which is:

[0080] Si: 0-0.40%, Fe: 0-0.80%, Cu: 2.0-2.6%, Mn: 0-0.30%, Mg: 1.2-2.9%, Cr: 0-0.50%, Zn: 5.1-8.3%, Ti: 0-0.15%; the remaining components are Al;

[0081] The aluminum alloy of the composition is subjected to the steps of the aluminum alloy sheet production method to obtain a rolled sheet. Multiple samples are taken from the rolled sheet, and the sampled sheets are processed respectively by changing some parameters using the steps of the aforementioned PLC defect elimination method. After the sample processing, the following tests are performed:

[0082] The surface morphology of the sample plate is detected by using a topological morphology analyzer;

[0083] The tissue morphology of the sample plate was detected using a transmission electron microscope (TEM);

[0084] The sample plates are respectively recorded as an embodiment and a comparative example. The differences between the processing steps of the two are listed below, and the similarities are not repeated here.

[0085] Example:

[0086] The temperature of the plate sample after quenching is 30°C. The permanent deformation of the plate after pre-stretching is 4.0%.

[0087] During the placement process and the pre-stretching process, the temperature of the plate sample is greater than 25°C.

[0088] The interval between quenching and pre-stretching of the plate specimen is 20 minutes.

[0089] Comparative Example:

[0090] The temperature of the plate sample after quenching is 8°C. The permanent deformation of the plate after pre-stretching is 2.0%.

[0091] During the placement process and the pre-stretching process, the temperature of the plate sample is less than 20°C.

[0092] The interval between quenching and pre-stretching of the plate specimen is 30 minutes.

[0093] Combination Figure 1 and Figure 2 The sample of the embodiment has no PLC defect on the surface, while the sample of the comparative example has obvious gully-shaped PLC defect. In addition, the permanent deformation of the sample of the embodiment is greater than that of the sample of the comparative example.

[0094] Recombination Figure 3 and Figure 4 After pre-stretching, the dislocation distribution of the samples of the embodiment is uniform and has no strip distribution. The dislocation movement does not show regular collective slip. Macroscopically, there is no PLC defect on the surface of the plate.

[0095] After pre-stretching, the sample of the comparative example has dislocations clustered in strip-like distribution, and the matrix of the strip-like dislocation wall moves. Macroscopically, PLC defects appear on the surface of the plate.

[0096] It can be seen that the aluminum alloy plate subjected to the PLC defect elimination method of the present invention increases the critical tensile deformation for the occurrence of PLC defects, and the critical tensile deformation is much larger than the 1.5-3.0% deformation specified in the pre-stretching treatment, meeting the standard requirements of the pre-stretching treatment.

[0097] In summary, the present invention provides a method for eliminating PLC defects, which controls the temperature of the aluminum alloy parts after quenching and cooling to not less than 25°C; maintains the activity of solute atoms, improves the pinning strength and pinning probability of solute atoms on movable dislocations, and makes it more difficult for solute atoms to get rid of pinning, thereby increasing the critical tensile deformation for the occurrence of PLC defects. PLC defects are avoided after pre-stretching. Compared with the long-term natural aging of the existing scheme, the present invention significantly shortens the interval time between quenching and pre-stretching treatment, avoids the increase of the yield strength of the aluminum alloy parts, and reduces the requirements for pre-stretching equipment. The production efficiency is improved and the qualified rate of the product surface quality is guaranteed. The present invention also provides a method for producing aluminum alloy plates, which are treated by the PLC defect elimination method to improve the surface quality of the plates.

[0098] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. A PLC defect elimination method, characterized in that: The steps include: S1, the aluminum alloy parts are solution treated and kept warm for a predetermined time; S2, the aluminum alloy parts are quenched and cooled; Control the temperature of aluminum alloy parts after quenching and cooling to no less than 25℃; S3, after quenching and cooling, the aluminum alloy part is placed for a predetermined period of time to perform pre-stretching treatment.

2. The PLC defect elimination method according to claim 1, characterized in that: During the placement process and the pre-stretching process, the temperature of the aluminum alloy part is not lower than 25°C.

3. The PLC defect elimination method according to claim 1, characterized in that: The aluminum alloy part is placed for no more than 24 hours after quenching and cooling.

4. The PLC defect elimination method according to claim 1, characterized in that: After quenching and cooling, the aluminum alloy part is placed for 20-30 minutes.

5. The PLC defect elimination method according to claim 1, characterized in that: The quenching and cooling process comprises: Hardening stage: The aluminum alloy parts are cooled rapidly, and a supersaturated solid solution structure is formed inside; Soft quenching stage: The temperature of the aluminum alloy part is further reduced, and its temperature is not lower than 25℃.

6. The PLC defect elimination method according to claim 5, characterized in that: In both the hard quenching section and the soft quenching section, the aluminum alloy parts are cooled by spraying cooling water; in the soft quenching section, the temperature of the sprayed cooling water is not less than 25°C.

7. The PLC defect elimination method according to claim 6, characterized in that: The spray cooling water used in the soft quenching section is obtained by mixing the water sprayed in the hard quenching section with cold water in a predetermined ratio; the temperature of the spray cooling water in the soft quenching section is controlled at 30°C.

8. A method for producing an aluminum alloy sheet, characterized in that: The steps include: Z1, casting heat-treatable strengthened aluminum alloy flat ingot; Z2, performing homogenization heat treatment on the aluminum alloy slab; Z3, heating the aluminum alloy flat ingot to 420° C., taking it out of the furnace and rolling it into a plate; Z4. Processing the plate by using the PLC defect elimination method as described in any one of claims 1 to 7.

9. The method for producing an aluminum alloy sheet according to claim 8, characterized in that: The aluminum alloy slab is subjected to homogenization heat treatment using a three-stage homogenization system, including: Heat to 400-405°C at a heating rate of ≥40°C / h and keep warm for 3h; Heat to 445-460℃ at a heating rate of ≥40℃ / h and keep warm for 10-24h; Heat to 485-496°C at a heating rate of ≥30°C / h and keep warm for 8-24h.

10. The method for producing an aluminum alloy sheet according to claim 8, wherein: The material of the aluminum alloy plate is: 2xxx, 6xxx or 7xxx series aluminum alloy.

Citation Information

Cited By

  • Preparation method of green low-carbon 7000 series aluminum plate strip for consumer electronics