Method for controlling primary alpha slice layer in TC18 titanium alloy die forging dual annealing process

Through the dual heat treatment system and a specific temperature time range, the formula is used to control the primary alpha sheet of TC18 titanium alloy die forgings, which solves the problem of failure to effectively control the alpha sheet in the prior art, and achieves accurate control of the quality and performance of the forgings and mechanical properties improve.

CN119082641APending Publication Date: 2024-12-06CHINA NAT ERZHONG GRP DEYANG WANHANG DIE FORGING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411255425.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art has failed to effectively control the primary alpha sheet layer of TC18 titanium alloy die forging during the double annealing process, affecting the quality and performance of the forging.

Method used

The dual heat treatment system is adopted, and the volume fraction of the primary α sheet is controlled by formula Vαp=0.83t2+32.2, and the thickness of the primary α sheet is controlled by formula Tαp=10.5/t1. The specific temperature and time range are 820~860℃. The second step is 740-760°C, and the insulation times t1 and t2 are between 0.5-4h and 0.5-6h, respectively.

Benefits of technology

Accurately adjust the content and size of primary α sheets, improve the mechanical properties of forgings, simplify the heat treatment process, and improve the accuracy of process design and simplify operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082641A_ABST
    Figure CN119082641A_ABST
Patent Text Reader

Abstract

The invention relates to a method for controlling a primary alpha lamella in a TC18 titanium alloy die forging dual annealing process, and belongs to the technical field of titanium alloy production. The control method for the primary alpha slice layer in the dual annealing process of the TC18 titanium alloy die forging comprises the steps that a dual heat treatment system is adopted for heat treatment in the production process of the TC18 titanium alloy die forging, and the dual heat treatment system comprises the steps that the temperature is increased to a first step along with a furnace, and heat preservation is conducted; then cooling to a second step along with the furnace for heat preservation, and finally performing air cooling; the temperature of the first step is 820-860 DEG C, and the temperature of the second step is 740-760 DEG C; the volume fraction V alpha p of the primary alpha sheet layer is controlled according to a formula (1): V alpha p = 0.83 t < 2 > + 32.2 # (1); in the formula, V alpha p is the volume fraction of the primary alpha phase, the unit is%, t2 is the heat preservation time of the second step, and the unit is h. According to the method, the content and the size of the primary alpha lamella can be regulated and controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for controlling a primary alpha sheet in a double annealing process of a TC18 titanium alloy die forging, and belongs to the technical field of titanium alloy production. Background Art

[0002] TC18 titanium alloy is a high-strength and high-toughness aviation titanium alloy, which is widely used in the structures of various aircraft. As a typical near-β-type titanium alloy, TC18 titanium alloy die forgings are heat treated using a double annealing heat treatment system, such as Figure 1 As shown in the figure, the forging is heated to the first step with the furnace and kept warm; then it is cooled to the second step with the furnace for keeping warm, and finally air-cooled. Since this system is relatively complex, improper control will have a great impact on the quality of the forging. It is of great significance to establish a clear method for regulating the content and size of the α sheet for the controllable manufacturing of forgings.

[0003] However, there is currently no method for controlling the primary α lamellae during the double annealing process of TC18 titanium alloy die forgings. Summary of the invention

[0004] The purpose of the present invention is to provide a method for controlling the primary alpha lamellae in the double annealing process of a TC18 titanium alloy die forging.

[0005] To achieve the purpose of the present invention, the method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging comprises:

[0006] The production process of TC18 titanium alloy die forgings adopts a double heat treatment system for heat treatment, which includes: heating to the first step with the furnace and keeping the temperature; then cooling to the second step with the furnace for keeping the temperature, and finally air cooling; the temperature of the first step is 820-860°C, and the temperature of the second step is 740-760°C;

[0007] The volume fraction V of the primary α-sheet αp Control according to formula (1):

[0008] V αp =0.83t2+32.2#(1);

[0009] Where V αp is the volume fraction of the primary α phase, unit: %, t2 is the holding time of the second step, unit: h.

[0010] According to the standard requirements of engineering manufacturing and the required range of α phase volume fraction, the holding time is calculated according to formula (1).

[0011] In a specific embodiment, the thickness of the primary α sheet is αp Control according to formula (2):

[0012]

[0013] Where T αp is the thickness of the primary α phase, unit: μm; t1 is the holding time of the first step, unit: h.

[0014] According to the standard requirements of engineering manufacturing and the required range of α phase thickness, the insulation time is calculated according to formula (2).

[0015] In a specific embodiment, the temperature of the first step is 830-860°C.

[0016] In a specific embodiment, the temperature of the first step is 835-860°C.

[0017] In a specific embodiment, the temperature of the second step is 740-755°C.

[0018] In a specific embodiment, the temperature of the second step is 740-750°C.

[0019] In a specific embodiment, the t1 is less than 5 h.

[0020] In a specific embodiment, the t2 is less than 6h.

[0021] In a specific embodiment, the 0.5≤t1≤4h.

[0022] In a specific embodiment, the 0.5≤t2≤4h.

[0023] Beneficial effects:

[0024] The present invention accurately establishes the influence of the second step holding time on the primary α lamella content, and the influence of the first step holding time on the primary α lamella thickness of the TC18 titanium alloy die forging. Through formula (1), formula (2) and the requirements of the mechanical properties of the forging for the primary α lamella, the heat treatment process of the die forging can be quickly calculated, providing support for the forging and process design, with the advantages of simple operation and accuracy, and realizing the regulation of the primary α lamella content and size. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a double heat treatment system diagram.

[0026] Figure 2 This is the geometric shape of the forging in Example 1.

[0027] Figure 3 This is the microstructure of the forging in Example 1. DETAILED DESCRIPTION

[0028] To achieve the purpose of the present invention, the method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging comprises:

[0029] The production process of TC18 titanium alloy die forgings adopts a double heat treatment system for heat treatment, which includes: heating to the first step with the furnace and keeping the temperature; then cooling to the second step with the furnace for keeping the temperature, and finally air cooling; the temperature of the first step is 820-860°C, and the temperature of the second step is 740-760°C;

[0030] The volume fraction V of the primary α-sheet αp Control according to formula (1):

[0031] V αp =0.83t2+32.2#(1);

[0032] Where V αp is the volume fraction of the primary α phase, unit: %, t2 is the holding time of the second step, unit: h.

[0033] According to the standard requirements of engineering manufacturing and the required range of α phase volume fraction, the holding time is calculated according to formula (1).

[0034] In a specific embodiment, the thickness of the primary α sheet is αp Control according to formula (2):

[0035]

[0036] Where T αp is the thickness of the primary α phase, unit: μm; t1 is the holding time of the first step, unit: h.

[0037] According to the standard requirements of engineering manufacturing and the required range of α phase thickness, the insulation time is calculated according to formula (2).

[0038] In a specific embodiment, the temperature of the first step is 830-860°C.

[0039] In a specific embodiment, the temperature of the first step is 835-860°C.

[0040] In a specific embodiment, the temperature of the second step is 740-755°C.

[0041] In a specific embodiment, the temperature of the second step is 740-750°C.

[0042] In a specific embodiment, the t1 is less than 5h.

[0043] In a specific embodiment, the t2 is less than 6h.

[0044] In a specific embodiment, the 0.5≤t1≤4h.

[0045] In a specific embodiment, the 0.5≤t2≤4h.

[0046] In one embodiment, a dual heat treatment system is shown in FIG. Figure 1 shown.

[0047] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0048] Example 1

[0049] A method for controlling the primary alpha lamellae of a TC18 large structural die forging for aircraft during double annealing, wherein the die forging has a geometric shape such as Figure 2 As shown, the details are as follows:

[0050] The forging needs to control the primary α content to about 34%, while maintaining the primary α thickness of 1.65μm, in order to ensure the tensile strength of the forging ≥1120MPa and the fracture toughness ≥75MPa.m 1 / 2

[0051] S1: primary α sheet thickness V αp is 34%. Substituting it into formula (1), it is calculated that the effective insulation time t2 required for the forging in the second step is not less than 2.2h;

[0052] S2: primary α sheet thickness T αp is 1.65 μm. Substituting it into formula (2), it is calculated that the effective insulation time t1 required for the forging in the first step is not less than 1.68 h;

[0053] S3: The forging was heat treated by double heat treatment system, the temperature of the first step was 845℃, the temperature of the second step was 740℃, and the actual effective heat preservation was 1.7h on the first step and 2.3h on the second step. The microstructure obtained is as follows Figure 3 As shown, after image recognition processing, the primary α ratio of the forging is calculated to be 34.6%, the sheet thickness is 1.70μm, and the mechanical properties of the forging are shown in Table 1.

[0054] Table 1 Mechanical properties test results of forgings of Example 1

[0055]

Claims

1. A method for controlling the primary α lamellae during double annealing of TC18 titanium alloy die forgings, characterized in that: The method comprises: The production process of TC18 titanium alloy die forgings adopts a double heat treatment system for heat treatment, which includes: heating to the first step with the furnace and keeping the temperature; then cooling to the second step with the furnace for keeping the temperature, and finally air cooling; the temperature of the first step is 820-860°C, and the temperature of the second step is 740-760°C; The volume fraction V of the primary α-sheet α p is controlled according to formula (1): V ap =0.83t2+32.2#(1); Where V αp is the volume fraction of the primary α phase, unit: %, t2 is the holding time of the second step, unit: h.

2. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1, characterized in that: The thickness of the primary α sheet is T αp Control according to formula (2): Where T α p is the thickness of the primary α phase, unit: μm; t1 is the insulation time of the first step, unit: h.

3. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The temperature of the first step is 830-860°C.

4. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The temperature of the first step is 835-860°C.

5. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The temperature of the second step is 740-755°C.

6. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The temperature of the second step is 740-750°C.

7. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The t1 is less than 5h.

8. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The t2 is less than 6h.

9. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The 0.5≤t1≤4h.

10. The method for controlling the primary α lamellae during the double annealing process of the TC18 titanium alloy die forging according to claim 1 or 2, characterized in that: The 0.5≤t2≤4h.