BG500 steel bearing part structure corrosion method

By using corrosive agents of potassium permanganate, concentrated sulfuric acid and water to corrode BG500 steel at 60-65°C or at room temperature, its grain size is revealed, solving the problem of corrosion manifestation of BG500 steel, and achieving satisfaction with level 6 or more grain size requirements.

CN119082737APending Publication Date: 2024-12-06HARBIN INST OF TECH +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411228102.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The excellent corrosion resistance of BG500 steel has difficulty in corrosion, and existing methods cannot effectively display its grain size.

Method used

The corrosion agent prepared by mixing potassium permanganate, concentrated sulfuric acid and water, with a mass-volume ratio of 1 g: (7-8)mL: (80-100)mL, and was carried out at 60-65°C for 10-15 minutes or at room temperature of 8- 12 hours of corrosion treatment.

Benefits of technology

A grain size corrosion method suitable for BG500 stainless steel was successfully provided. The grain size of the grain size meets the requirements of 6 levels or finer, solving the problem of corrosion display difficulties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082737A_ABST
    Figure CN119082737A_ABST
Patent Text Reader

Abstract

The invention relates to a BG500 steel bearing part structure corrosion method, and aims to solve the problem that grain size corrosion is difficult to appear due to excellent corrosion resistance of existing BG500 steel. The method comprises the steps that firstly, a corrosive agent is prepared, and the corrosive agent is formed by mixing potassium permanganate, concentrated sulfuric acid and water; the mass volume ratio of potassium permanganate to concentrated sulfuric acid to water is 1g: (7-8) mL: (80-100) mL; secondly, a BG500 steel bearing sample is soaked in the corrosive agent and then corroded, and if the BG500 steel bearing sample is corroded at the temperature of 60-65 DEG C, the corrosion time ranges from 10 min to 15 min; and if normal-temperature corrosion is carried out, the corrosion time is 8-12 hours. According to the method, the grain size problem of the BG500 stainless steel is solved, and the grain size meets the 6-level or finer requirement. The method is applied to the field of BG500 steel bearing part structure corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for organizing corrosion of a BG500 steel bearing part. Background Art

[0002] The average grain size has a great influence on the strength, plasticity and other performance indicators of the material. It is an important indicator in the technical requirements of metal materials. The determination of the average grain size is a widely used test item in metallographic inspection.

[0003] In the 1990s, the United States developed high nitrogen stainless bearing steel, which reduced the carbon content and added nitrogen to the traditional high carbon martensitic stainless steel, and formulated the American aviation material standard AMS5925. At present, this material has been widely used in aviation bearings with corrosion resistance requirements in Europe and the United States. The steel is evenly distributed with very small granular carbonitrides formed by nitrogen and carbon, without the coarse eutectic carbides and needle-shaped eutectic carbides in high carbon stainless steel. In addition, because nitrogen strengthens martensite, its toughness, corrosion resistance and fatigue performance are better than those of traditional high carbon chromium stainless bearing steel.

[0004] BG500 steel is a nitrogen-containing martensitic stainless steel with much higher corrosion resistance than traditional high-carbon chromium stainless bearing steel. The addition of nitrogen can effectively reduce the ferrite content in the steel, make the austenite more stable, and delay the precipitation time of M23C6, greatly improving the corrosion resistance of high nitrogen steel. Conventional nitric acid + alcohol corrosive agents will form a passivation layer on the surface of high nitrogen steel, resulting in the inability to show the grain size. Summary of the invention

[0005] The purpose of the present invention is to solve the problem that the existing BG500 steel has excellent corrosion resistance but grain size corrosion is difficult to show, and a method for organizing corrosion of BG500 steel bearing parts is provided.

[0006] A method for structural corrosion of a BG500 steel bearing part of the present invention is carried out in the following steps:

[0007] 1. preparing an etchant, wherein the etchant is a mixture of potassium permanganate, concentrated sulfuric acid and water; the mass volume ratio of potassium permanganate, concentrated sulfuric acid and water is 1 g: (7-8) mL: (80-100) mL;

[0008] 2. Soak the BG500 steel bearing sample in the corrosive agent and then corrode it. If the corrosion is carried out at 60-65°C, the corrosion time is 10-15 minutes; if the corrosion is carried out at room temperature, the corrosion time is 8-12 hours.

[0009] Beneficial effects of the present invention:

[0010] The present invention successfully provides a grain size corrosion method suitable for BG500 stainless steel by adjusting the composition of the corrosive agent and the corrosion method, solves the problem that the grain size corrosion of BG500 stainless steel is difficult to show, and the grain size meets the requirements of level 6 or finer. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is the actual grain size diagram of BG500. DETAILED DESCRIPTION

[0012] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0013] Specific implementation method 1: In this implementation method, a BG500 steel bearing part tissue corrosion method is carried out according to the following steps:

[0014] 1. preparing an etchant, wherein the etchant is a mixture of potassium permanganate, concentrated sulfuric acid and water; the mass volume ratio of potassium permanganate, concentrated sulfuric acid and water is 1 g: (7-8) mL: (80-100) mL;

[0015] 2. Soak the BG500 steel bearing sample in the corrosive agent and then corrode it. If the corrosion is carried out at 60-65°C, the corrosion time is 10-15 minutes; if the corrosion is carried out at room temperature, the corrosion time is 8-12 hours.

[0016] This embodiment successfully provides a grain size corrosion method suitable for BG500 stainless steel by adjusting the composition of the corrosive agent and the corrosion method, solving the problem that the grain size corrosion of BG500 stainless steel is difficult to show, and the grain size meets the requirements of level 6 or finer.

[0017] Specific implementation method 2: This implementation method is different from the specific implementation method 1 in that the mass concentration of concentrated sulfuric acid is ≥ 98%. Other aspects are the same as the specific implementation method 1.

[0018] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the mass volume ratio of potassium permanganate, concentrated sulfuric acid and water is 1 g:7.5 mL:90 mL. The rest is the same as specific implementation method 1 or 2.

[0019] Specific implementation method 4: This implementation method is different from specific implementation methods 1 to 3 in that the size of the G500 steel bearing sample is 20±1 mm. Other aspects are the same as those of specific implementation methods 1 to 3.

[0020] Specific implementation mode 5: This implementation mode is different from the specific implementation modes 1 to 4 in that the etching is performed at 62° C. for 12 minutes in step 2. The rest is the same as the specific implementation modes 1 to 4.

[0021] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that the etching is performed at room temperature for 10 hours in step 2. The rest is the same as specific implementation methods 1 to 5.

[0022] The following examples are used to verify the beneficial effects of the present invention.

[0023] Embodiment 1: In this embodiment, a method for corrosion of a BG500 steel bearing part is carried out according to the following steps:

[0024] 1. preparing an etchant, wherein the etchant is a mixture of potassium permanganate, concentrated sulfuric acid and water; the mass volume ratio of potassium permanganate, concentrated sulfuric acid and water is 1g:7.5mL:90mL;

[0025] 2. Immerse the BG500 steel bearing sample in the corrosive agent and then corrode it at room temperature. The corrosion time is 10 hours.

[0026] The corroded BG500 steel bearing specimens were tested. Figure 1 This is the actual grain size diagram of BG500 in this embodiment; it can be seen from the figure that the actual grain size of BG500 can reach level 8.

[0027] Comparative Example:

[0028] The conventional bearing parts grain size corrosion method was used to corrode the BG500 steel bearing sample. The specific method is: 3-4% nitric acid ethanol solution or 5% picric acid ethanol solution is used to soak the sample for 10 minutes and then dry it to check the polished surface. The test results show that due to the corrosion resistance of BG500 stainless steel, the grains cannot be seen.

Claims

1. A method for the corrosion of BG500 steel bearing parts, characterized in that The method proceeds as follows:

1. preparing an etchant, wherein the etchant is a mixture of potassium permanganate, concentrated sulfuric acid and water; the mass volume ratio of potassium permanganate, concentrated sulfuric acid and water is 1 g: (7-8) mL: (80-100) mL; 2. Soak the BG500 steel bearing sample in the corrosive agent and then corrode it. If the corrosion is carried out at 60-65°C, the corrosion time is 10-15 minutes; if the corrosion is carried out at room temperature, the corrosion time is 8-12 hours.

2. A method for structural corrosion of BG500 steel bearing parts according to claim 1, characterized in that: The mass concentration of concentrated sulfuric acid is ≥98%.

3. The method for structural corrosion of BG500 steel bearing parts according to claim 1, characterized in that: The mass volume ratio of potassium permanganate, concentrated sulfuric acid and water is 1g:7.5mL:90mL.

4. The method for structural corrosion of BG500 steel bearing parts according to claim 1, characterized in that: The specimen size of BG500 steel bearing is 20±1mm.

5. The method for structural corrosion of BG500 steel bearing parts according to claim 1, characterized in that: In step 2, the corrosion is carried out at 62°C for 12 minutes.

6. A method for structural corrosion of BG500 steel bearing parts according to claim 1, characterized in that: In step 2, the corrosion is carried out at room temperature for 10 hours.

Citation Information

Patent Citations

  • Method for displaying original austenite grain boundary of 40Cr15Mo2VN bearing steel

    CN102221495A

  • Corrosion method capable of displaying original austenite grain boundary of high-nitrogen martensite stainless steel

    CN107014661A

  • Corrosion method of bearing steel grain size

    CN110132697A

  • Precipitation-strengthened martensitic stainless steel original austenite grain boundary corrosion method

    CN111638113A

  • Corrosive agent for displaying austenite grain boundary of martensitic stainless steel and display method

    CN112304733A