Multifunctional corrosion inhibitor and preparation method thereof
By designing a multifunctional corrosion inhibitor containing main corrosion inhibitor, polyaniline coated with modified graphene oxide and other components, the problems of reduced efficiency and poor stability of traditional corrosion inhibitors at high temperatures are solved, and the high temperature environment is achieved The excellent corrosion inhibition and corrosion resistance under the umbrella are suitable for modern industrial needs.
Patent Information
- Application Number
- CN202411212122.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional corrosion inhibitors show reduced corrosion inhibition efficiency and poor stability under high temperature conditions, which is difficult to meet the strict requirements of modern industry for corrosion protection.
A multifunctional corrosion inhibitor is used, and its formulation includes the main corrosion inhibitor, polyaniline coated modified graphene oxide, propyne alcohol, sodium dodecyl benzene sulfonate, N,N-dimethylformamide and Anhydrous ethanol, through specific chemical structure design and process treatment, ensures excellent corrosion inhibition and corrosion resistance under high temperature environments.
This multi-functional corrosion inhibitor maintains stability and durability under high temperature conditions, effectively inhibits metal corrosion, extends the service life of the equipment, and has functions such as scale inhibition and dispersion. It is suitable for different types of metals and various corrosion media, improving equipment operation Efficiency, easy to control the process and low cost.
Smart Images

Figure BDA0005020565700000191
Abstract
Description
Technical Field
[0001] The invention relates to the field of corrosion inhibitors, and in particular to a multifunctional corrosion inhibitor and a preparation method thereof. Background Art
[0002] In the process of oil and gas field development, acidizing technology is a commonly used measure to increase production. During acidizing construction, high-concentration hydrochloric acid is usually squeezed into the formation to corrode the rock and increase the oil and gas channel, thereby achieving the purpose of increasing production. However, under the condition of high acid concentration, the risk of acid corrosion on metal materials will increase significantly, resulting in reduced equipment performance, shortened life, and even safety accidents. The most common solution is to add corrosion inhibitors.
[0003] Corrosion inhibitors, also known as corrosion inhibitors, are chemical substances or compounds that exist in a corrosive environment in an appropriate concentration and form and can prevent or slow down the corrosion of materials. Corrosion inhibitors have the characteristics of low cost, simple operation, quick effect, and suitability for long-term use. However, traditional corrosion inhibitors often show the disadvantages of decreased corrosion inhibition efficiency and poor stability, especially under high temperature conditions, and are difficult to meet the strict requirements of modern industry for corrosion protection. Therefore, it is of great significance to develop a multifunctional corrosion inhibitor and its preparation method that can maintain high-efficiency corrosion inhibition performance under various temperature conditions, especially high temperature conditions. Summary of the invention
[0004] In order to overcome the above technical problems, the purpose of the present invention is to provide a multifunctional corrosion inhibitor and a preparation method thereof, which solves the problems of reduced corrosion inhibition efficiency and poor stability of traditional corrosion inhibitors under high temperature conditions.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A multifunctional corrosion inhibitor comprises the following components in parts by weight:
[0007] 75-85 parts of main corrosion inhibitor, 3.8-11.6 parts of polyaniline-coated modified graphene oxide, 4.2-8.8 parts of propargyl alcohol, 1.2-2.6 parts of sodium dodecylbenzene sulfonate, 45-55 parts of N,N-dimethylformamide, 30-40 parts of anhydrous ethanol and 33-55 parts of deionized water;
[0008] Wherein, the main corrosion inhibitor is prepared by the following steps:
[0009] Step A1: 2-chloro-5-nitrotrifluorotoluene, ethylene glycol, urea and dichloromethane are added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 25-30° C. and a stirring rate of 300-400 r / min for 20-25 min, and then the temperature is raised to 80-85° C. and the stirring reaction is continued for 2-3 h. After the reaction is completed, the reaction product is cooled to room temperature, and then added to distilled water, and then extracted with ethyl acetate for 2-3 times. The extracts are combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;
[0010] Step A2: Add intermediate 1, 5% palladium carbon and anhydrous ethanol to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, stir and react for 20-25 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then introduce hydrogen to maintain the pressure at 4-5MPa and continue stirring and reacting for 3-5 hours at a temperature of 60-65°C. After the reaction is completed, the reaction product is cooled to room temperature, then vacuum filtered, the filtrate is added to ice water and allowed to stand for precipitation, then vacuum filtered, the filter cake is placed in a vacuum drying oven, and dried at a temperature of 60-65°C for 3-5 hours to obtain intermediate 2;
[0011] Step A3: Add intermediate 2, epichlorohydrin and tetrabutylammonium bromide to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, introduce nitrogen protection, stir and react for 20-25 minutes at a temperature of 25-30° C. and a stirring rate of 300-400 r / min, then heat to 75-80° C. and continue stirring and reacting for 2-4 hours. After the reaction is completed, cool the reaction product to room temperature, and then distill off excess epichlorohydrin under reduced pressure to obtain intermediate 3;
[0012] Step A4: Add the intermediate 3, 4-methylquinoline and anhydrous ethanol to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 20-25 minutes at a temperature of 25-30°C and a stirring rate of 300-400r / min, then raise the temperature to reflux and continue stirring the reaction for 4-5 hours. After the reaction is completed, the reaction product is cooled to room temperature, and then the solvent is removed by rotary evaporation to obtain the main corrosion inhibitor.
[0013] As a further solution of the present invention: the usage ratio of the 2-chloro-5-nitrotrifluorotoluene, ethylene glycol, urea and dichloromethane in step A1 is 20 mmol: 10 mmol: 1-2 mmol: 50-60 mL.
[0014] As a further solution of the present invention: the usage ratio of the intermediate 1, 5% palladium carbon and anhydrous ethanol in step A2 is 10 mmol: 0.25-0.45 g: 50-60 mL.
[0015] As a further solution of the present invention: the usage ratio of the intermediate 2, epichlorohydrin and tetrabutylammonium bromide in step A3 is 10 mmol: 120-140 mmol: 0.5-1.5 g.
[0016] As a further solution of the present invention: the usage ratio of the intermediate 3, 4-methylquinoline and anhydrous ethanol in step A4 is 10 mmol:40 mmol:60-80 mL.
[0017] As a further solution of the present invention: the polyaniline-coated modified graphene oxide is prepared by the following steps:
[0018] Step B1: Add graphite powder, concentrated sulfuric acid and sodium nitrate to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, introduce nitrogen protection, stir and react for 30-50 minutes at a temperature of 0-5°C and a stirring rate of 300-400r / min, then add potassium permanganate and continue to stir and react for 1-1.5 hours at a temperature of 35-40°C, then continue to stir and react for 1-1.5 hours at a temperature of 95-100°C, pour the reaction product into ice water after the reaction is completed, then add hydrogen peroxide solution, then stand for 8-10 hours, then centrifuge, wash the precipitate with hydrochloric acid solution and distilled water for 3-5 times in sequence, then place it in a vacuum drying oven, and dry it at a temperature of 45-50°C for 5-6 hours to obtain graphene oxide;
[0019] Step B2: adding graphene oxide and N, N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, ultrasonically treating for 1-2 hours at an ultrasonic frequency of 40-50kHz, then adding diethylenetriamine and stirring the reaction for 10-15 hours at a temperature of 60-65°C and a stirring rate of 300-400r / min. After the reaction is completed, the reaction product is cooled to room temperature and then centrifuged. The precipitate is washed with distilled water for 3-5 times, and then placed in a vacuum drying oven and dried at a temperature of 45-50°C for 3-4 hours to obtain amino-modified graphene oxide;
[0020] Step B3: Add amino-modified graphene oxide, sodium dodecylbenzene sulfonate and deionized water to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and perform ultrasonic treatment for 1-2 hours at an ultrasonic frequency of 40-50kHz, then adjust the pH to 1-2 with a hydrochloric acid solution, then add aniline and ammonium persulfate and stir the reaction at a temperature of 0-5°C and a stirring rate of 300-400r / min for 8-10 hours. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed with anhydrous ethanol and distilled water for 3-5 times in sequence, and then placed in a vacuum drying oven and dried at a temperature of 45-50°C for 6-8 hours to obtain polyaniline-coated modified graphene oxide.
[0021] As a further solution of the present invention: the usage ratio of the graphite powder, concentrated sulfuric acid, sodium nitrate, potassium permanganate and hydrogen peroxide solution in step B1 is 1 g: 20-30 mL: 0.5-0.7 g: 4.5-5.5 g: 2-3 mL.
[0022] As a further solution of the present invention: in step B1, the mass fraction of the concentrated sulfuric acid is 98%, the mass fraction of the hydrogen peroxide solution is 30%, and the mass fraction of the hydrochloric acid solution is 5-7%.
[0023] As a further solution of the present invention: the usage ratio of the graphene oxide, N,N-dimethylformamide and diethylenetriamine in step B2 is 1g:30-35mL:10-15g.
[0024] As a further solution of the present invention: the usage ratio of the amino-modified graphene oxide, sodium dodecylbenzenesulfonate, deionized water, aniline and ammonium persulfate in step B3 is 1g: 0.1-0.3g: 40-50mL: 1-2g: 1.8-2.2g.
[0025] As a further solution of the present invention: the mass fraction of the hydrochloric acid solution in step B3 is 20-25%.
[0026] As a further solution of the present invention: a method for preparing a multifunctional corrosion inhibitor comprises the following steps:
[0027] Step 1: weigh 75-85 parts of main corrosion inhibitor, 3.8-11.6 parts of polyaniline-coated modified graphene oxide, 4.2-8.8 parts of propargyl alcohol, 1.2-2.6 parts of sodium dodecylbenzene sulfonate, 45-55 parts of N,N-dimethylformamide, 30-40 parts of anhydrous ethanol and 33-55 parts of deionized water according to weight parts, and set aside;
[0028] Step 2: Add the main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 2-3 hours at a temperature of 60-65°C and a stirring rate of 300-400r / min to obtain a multifunctional corrosion inhibitor.
[0029] Beneficial effects of the present invention:
[0030] The invention discloses a multifunctional corrosion inhibitor and a preparation method thereof. The multifunctional corrosion inhibitor is obtained by adding a main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer for stirring and reacting. The multifunctional corrosion inhibitor ensures its stability and durability at various temperatures, especially in high-temperature environments, through special formula design and chemical structure design. Even under high-temperature conditions, the multifunctional corrosion inhibitor can maintain its excellent corrosion inhibition and anti-corrosion properties, can effectively inhibit metal corrosion in various temperature environments, especially in high-temperature environments, and prolong the service life of metal equipment. The multifunctional corrosion inhibitor has excellent high-temperature corrosion inhibition performance and wide applicability, and can be used for different types of metals and a variety of corrosive media. The multifunctional corrosion inhibitor also has certain scale inhibition, dispersion and other functions, and can improve the operation efficiency of the equipment. The process is easy to control, simple to operate, suitable for industrial production, and low in cost, with good economic benefits and application prospects.
[0031] In the process of preparing the multifunctional corrosion inhibitor, a main corrosion inhibitor is first prepared. First, 2-chloro-5-nitrotrifluorotoluene and ethylene glycol are reacted. The chlorine atom on the 2-chloro-5-nitrotrifluorotoluene reacts with the hydroxyl group on the ethylene glycol to form an intermediate 1 containing two nitro groups and a trifluoromethyl group. Then, the intermediate 1 reacts under hydrogen conditions, and the nitro group on it is reduced to an amino group to obtain an intermediate 2. Then, the intermediate 2 reacts with epichlorohydrin, and the amino group on the intermediate 2 reacts with the epoxy group on the epichlorohydrin to undergo a ring-opening reaction, introducing a chlorine atom and a hydroxyl group to obtain an intermediate 3. Then, the intermediate 3 reacts with 4-methylquinoline to obtain an intermediate 2. The chlorine atoms on the body 3 react with the tertiary amine group in 4-methylquinoline to form a quaternary ammonium group to obtain a main corrosion inhibitor; the molecular structure of the main corrosion inhibitor contains a large number of quaternary ammonium groups, which can be adsorbed on the metal surface through electrostatic attraction, hydrogen bonding and the like to form a protective film, blocking the contact between the corrosive medium and the metal, and changing the charge distribution on the metal surface, reducing the activity of the metal, thereby slowing down the corrosion reaction. The molecular structure of the main corrosion inhibitor also contains a trifluoromethyl group, and the fluorine-containing group has a lower surface energy, which can enhance the high-temperature stability and corrosion resistance of the protective film, further slow down the corrosion process, and enhance its high-temperature corrosion inhibition effect.
[0032] In the process of preparing the multifunctional corrosion inhibitor, a polyaniline-coated modified graphene oxide is also prepared. First, graphite powder is used as a raw material to prepare graphene oxide. Then, diethylenetriamine is used to modify the graphene oxide, and a large number of amino groups and imino groups are introduced on the surface of the graphene oxide particles to obtain amino-modified graphene oxide. Finally, aniline is used as a polymerization monomer to graft polyaniline on the surface of the amino-modified graphene oxide particles to coat the amino-modified graphene oxide to obtain polyaniline-coated modified graphene oxide. The graphene oxide in the polyaniline-coated modified graphene oxide has a unique two-dimensional sheet structure and can form a solid physical barrier on the metal surface, which can not only effectively block the penetration of corrosive media, but also pass through its nanostructured carbon nanotubes. Size effect, reducing the adsorption and diffusion of corrosive media, thereby enhancing the anti-corrosion effect. The polyaniline in the polyaniline-coated modified graphene oxide itself has good chemical stability and passivation properties, and can form a stable passivation film on the metal surface. This film can further inhibit the electrochemical corrosion reaction on the metal surface and improve the corrosion resistance of the metal. Therefore, the composite of polyaniline and graphene oxide not only retains their respective advantages, but also enhances the overall anti-corrosion performance through a synergistic effect. The two-dimensional layer structure of graphene oxide provides more attachment points for polyaniline, so that polyaniline can be more evenly distributed on the metal surface, and the presence of polyaniline can enhance the bonding force between graphene oxide and the metal surface, thereby improving the stability and durability of the composite coating. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Embodiment 1:
[0035] This embodiment is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0036] Step S1: 20 mmol 2-chloro-5-nitrotrifluorotoluene, 10 mmol ethylene glycol, 1 mmol urea and 50 mL dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 300 r / min for 20 min, and then the mixture was heated to 80° C. and the stirring reaction was continued for 2 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted twice with ethyl acetate, the extracts were combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0037] Step S2: 10 mmol of intermediate 1, 0.25 g of 5% palladium carbon and 50 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 20 min, and then hydrogen was introduced to maintain the pressure at 4 MPa and the temperature was raised to 60° C. and continued to stir for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filtrate was added to ice water and allowed to stand for precipitation, and then vacuum filtered, the filter cake was placed in a vacuum drying oven, and dried at a temperature of 60° C. for 3 h to obtain intermediate 2;
[0038] Step S3: 10 mmol of intermediate 2, 120 mmol of epichlorohydrin and 0.5 g of tetrabutylammonium bromide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 25° C. and a stirring rate of 300 r / min for 20 min, and then the temperature was raised to 75° C. and the stirring reaction was continued for 2 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the excess epichlorohydrin was distilled off under reduced pressure to obtain intermediate 3;
[0039] Step S4: 10 mmol of intermediate 3, 40 mmol of 4-methylquinoline and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 20 min, and then the temperature was raised to reflux and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0040] Step S5: 1 g of graphite powder, 20 mL of 98% concentrated sulfuric acid and 0.5 g of sodium nitrate are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The reaction is stirred for 30 min at a temperature of 0° C. and a stirring rate of 300 r / min, and then 4.5 g of potassium permanganate is added and the temperature is raised to 35° C. and the stirring reaction is continued for 1 h, and then the temperature is raised to 95° C. and the stirring reaction is continued for 1 h. After the reaction is completed, the reaction product is poured into ice water, and then 2 mL of 30% hydrogen peroxide solution is added, and then it is allowed to stand for 8 h, and then centrifuged. The precipitate is washed 3 times with a 5% hydrochloric acid solution and distilled water in sequence, and then placed in a vacuum drying oven and dried at a temperature of 45° C. for 5 h to obtain graphene oxide;
[0041] Step S6: 1 g of graphene oxide and 30 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 1 h at an ultrasonic frequency of 40 kHz, and then 10 g of diethylenetriamine was added and stirred for 10 h at a temperature of 60° C. and a stirring rate of 300 r / min. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was washed with distilled water for 3 times, and then placed in a vacuum drying oven and dried at a temperature of 45° C. for 3 h to obtain amino-modified graphene oxide;
[0042] Step S7: 1 g of amino-modified graphene oxide, 0.1 g of sodium dodecylbenzene sulfonate and 40 mL of deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 1 h at an ultrasonic frequency of 40 kHz, and then the pH is adjusted to 2 with a 20% hydrochloric acid solution, and then 1 g of aniline and 1.8 g of ammonium persulfate are added and stirred for 8 h at a temperature of 0°C and a stirring rate of 300 r / min. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed 3 times with anhydrous ethanol and distilled water in sequence, and then placed in a vacuum drying oven and dried at a temperature of 45°C for 6 h to obtain polyaniline-coated modified graphene oxide;
[0043] Step S8: weigh 75 parts of a main corrosion inhibitor, 3.8 parts of polyaniline-coated modified graphene oxide, 4.2 parts of propargyl alcohol, 1.2 parts of sodium dodecylbenzene sulfonate, 45 parts of N,N-dimethylformamide, 30 parts of anhydrous ethanol and 33 parts of deionized water according to weight parts, and set aside;
[0044] Step S9: Add the main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 2 hours at a temperature of 60° C. and a stirring rate of 300 r / min to obtain a multifunctional corrosion inhibitor.
[0045] Embodiment 2:
[0046] This embodiment is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0047] Step S1: 20 mmol 2-chloro-5-nitrotrifluorotoluene, 10 mmol ethylene glycol, 1.5 mmol urea and 55 mL dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 28° C. and a stirring rate of 350 r / min for 22 min, and then the mixture was heated to 82° C. and the stirring reaction was continued for 2.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with ethyl acetate twice, the extracts were combined and dried over anhydrous sodium sulfate, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0048] Step S2: 10 mmol of intermediate 1, 0.35 g of 5% palladium carbon and 55 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and stirred for reaction at a temperature of 28° C. and a stirring rate of 350 r / min for 22 min, and then hydrogen was introduced to maintain the pressure at 4.5 MPa and the temperature was raised to 62° C. and continued to stir for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filtrate was added to ice water and allowed to stand for precipitation, and then vacuum filtered, the filter cake was placed in a vacuum drying oven, and dried at a temperature of 62° C. for 4 h to obtain intermediate 2;
[0049] Step S3: 10 mmol of intermediate 2, 130 mmol of epichlorohydrin and 1 g of tetrabutylammonium bromide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 28° C. and a stirring rate of 350 r / min for 22 min, and then the mixture was heated to 78° C. and stirred for 3 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the excess epichlorohydrin was distilled off under reduced pressure to obtain intermediate 3;
[0050] Step S4: 10 mmol of intermediate 3, 40 mmol of 4-methylquinoline and 70 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for 22 min at a temperature of 28 ° C and a stirring rate of 350 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 4.5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0051] Step S5: 1 g of graphite powder, 25 mL of 98% concentrated sulfuric acid and 0.6 g of sodium nitrate are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The reaction is stirred for 40 min at a temperature of 3 ° C and a stirring rate of 350 r / min, and then 5 g of potassium permanganate is added and the temperature is raised to 38 ° C and the stirring reaction is continued for 1.2 h, and then the temperature is raised to 98 ° C and the stirring reaction is continued for 1.2 h. After the reaction is completed, the reaction product is poured into ice water, and then 2.5 mL of 30% hydrogen peroxide solution is added, and then it is allowed to stand for 9 h, and then centrifuged. The precipitate is washed 4 times with a 6% hydrochloric acid solution and distilled water in turn, and then placed in a vacuum drying oven and dried at a temperature of 48 ° C for 5.5 h to obtain graphene oxide;
[0052] Step S6: 1 g of graphene oxide and 32 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 1.5 h at an ultrasonic frequency of 45 kHz, and then 12 g of diethylenetriamine was added and stirred for 12 h at a temperature of 62 ° C and a stirring rate of 350 r / min. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was washed with distilled water 4 times, and then placed in a vacuum drying oven and dried at a temperature of 48 ° C for 3.5 h to obtain amino-modified graphene oxide;
[0053] Step S7: 1 g of amino-modified graphene oxide, 0.2 g of sodium dodecylbenzene sulfonate and 45 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 1.5 h at an ultrasonic frequency of 45 kHz, and then the pH was adjusted to 1.5 with a 22% hydrochloric acid solution, and then 1.5 g of aniline and 2 g of ammonium persulfate were added and stirred for 9 h at a temperature of 3 ° C and a stirring rate of 350 r / min. After the reaction was completed, the reaction product was centrifuged, and the precipitate was washed 4 times with anhydrous ethanol and distilled water in turn, and then placed in a vacuum drying oven and dried at a temperature of 48 ° C for 7 h to obtain polyaniline-coated modified graphene oxide;
[0054] Step S8: 80 parts of a main corrosion inhibitor, 7.7 parts of polyaniline-coated modified graphene oxide, 6.5 parts of propargyl alcohol, 1.9 parts of sodium dodecylbenzene sulfonate, 50 parts of N,N-dimethylformamide, 35 parts of anhydrous ethanol and 44 parts of deionized water were weighed in parts by weight for later use;
[0055] Step S9: Add the main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 2.5 hours at a temperature of 62° C. and a stirring rate of 350 r / min to obtain a multifunctional corrosion inhibitor.
[0056] Embodiment 3:
[0057] This embodiment is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0058] Step S1: 20 mmol 2-chloro-5-nitrotrifluorotoluene, 10 mmol ethylene glycol, 2 mmol urea and 60 mL dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 30° C. and a stirring rate of 400 r / min for 25 min, and then the mixture was heated to 85° C. and stirred for 3 h. After the reaction, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with ethyl acetate for 3 times. The extracts were combined and dried over anhydrous sodium sulfate, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0059] Step S2: 10 mmol of intermediate 1, 0.45 g of 5% palladium carbon and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then hydrogen was introduced to maintain the pressure at 5 MPa and the temperature was raised to 65° C. and continued to stir for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filtrate was added to ice water and allowed to stand for precipitation, and then vacuum filtered, the filter cake was placed in a vacuum drying oven, and dried at a temperature of 65° C. for 5 h to obtain intermediate 2;
[0060] Step S3: 10 mmol of intermediate 2, 140 mmol of epichlorohydrin and 1.5 g of tetrabutylammonium bromide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to 80° C. and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the excess epichlorohydrin was distilled off under reduced pressure to obtain intermediate 3;
[0061] Step S4: 10 mmol of intermediate 3, 40 mmol of 4-methylquinoline and 80 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to reflux and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0062] Step S5: 1 g of graphite powder, 30 mL of 98% concentrated sulfuric acid and 0.7 g of sodium nitrate are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 5° C. and a stirring rate of 400 r / min for 50 min, and then 5.5 g of potassium permanganate is added and the mixture is stirred for reaction for 1.5 h at a temperature of 40° C., and then the mixture is stirred for reaction for 1.5 h at a temperature of 100° C. After the reaction is completed, the reaction product is poured into ice water, and then 3 mL of 30% hydrogen peroxide solution is added, and the mixture is allowed to stand for 10 h, and then centrifuged. The precipitate is washed 5 times with a 7% hydrochloric acid solution and distilled water, and then placed in a vacuum drying oven and dried at a temperature of 50° C. for 6 h to obtain graphene oxide;
[0063] Step S6: 1 g of graphene oxide and 35 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 2 h at an ultrasonic frequency of 50 kHz, then 15 g of diethylenetriamine was added and stirred for 15 h at a temperature of 65 ° C and a stirring rate of 400 r / min. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was washed with distilled water for 5 times, and then placed in a vacuum drying oven and dried at a temperature of 50 ° C for 4 h to obtain amino-modified graphene oxide;
[0064] Step S7: 1 g of amino-modified graphene oxide, 0.3 g of sodium dodecylbenzene sulfonate and 50 mL of deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 2 h at an ultrasonic frequency of 50 kHz, and then the pH is adjusted to 1 with a 25% hydrochloric acid solution, and then 2 g of aniline and 2.2 g of ammonium persulfate are added and stirred for 10 h at a temperature of 5 ° C and a stirring rate of 400 r / min. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed 5 times with anhydrous ethanol and distilled water in turn, and then placed in a vacuum drying oven and dried at a temperature of 50 ° C for 8 h to obtain polyaniline-coated modified graphene oxide;
[0065] Step S8: 85 parts of a main corrosion inhibitor, 11.6 parts of polyaniline-coated modified graphene oxide, 8.8 parts of propargyl alcohol, 2.6 parts of sodium dodecylbenzene sulfonate, 55 parts of N,N-dimethylformamide, 40 parts of anhydrous ethanol and 55 parts of deionized water were weighed in parts by weight for later use;
[0066] Step S9: Add the main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 3 hours at a temperature of 65° C. and a stirring rate of 400 r / min to obtain a multifunctional corrosion inhibitor.
[0067] Comparative Example 1:
[0068] This comparative example is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0069] Step S1: 10 mmol benzyl chloride, 40 mmol 4-methylquinoline and 80 mL anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to reflux and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0070] Step S2: weigh 85 parts of a main corrosion inhibitor, 8.8 parts of propargyl alcohol, 2.6 parts of sodium dodecylbenzene sulfonate, 55 parts of N,N-dimethylformamide, 40 parts of anhydrous ethanol and 55 parts of deionized water according to weight parts, and set aside;
[0071] Step S3: Add the main corrosion inhibitor, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 3 hours at a temperature of 65° C. and a stirring rate of 400 r / min to obtain a multifunctional corrosion inhibitor.
[0072] Comparative Example 2:
[0073] This comparative example is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0074] Step S1: 20 mmol 2-chloro-5-nitrotrifluorotoluene, 10 mmol ethylene glycol, 2 mmol urea and 60 mL dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 30° C. and a stirring rate of 400 r / min for 25 min, and then the mixture was heated to 85° C. and stirred for 3 h. After the reaction, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with ethyl acetate for 3 times. The extracts were combined and dried over anhydrous sodium sulfate, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0075] Step S2: 10 mmol of intermediate 1, 0.45 g of 5% palladium carbon and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then hydrogen was introduced to maintain the pressure at 5 MPa and the temperature was raised to 65° C. and continued to stir for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filtrate was added to ice water and allowed to stand for precipitation, and then vacuum filtered, the filter cake was placed in a vacuum drying oven, and dried at a temperature of 65° C. for 5 h to obtain intermediate 2;
[0076] Step S3: 10 mmol of intermediate 2, 140 mmol of epichlorohydrin and 1.5 g of tetrabutylammonium bromide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to 80° C. and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the excess epichlorohydrin was distilled off under reduced pressure to obtain intermediate 3;
[0077] Step S4: 10 mmol of intermediate 3, 40 mmol of 4-methylquinoline and 80 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to reflux and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0078] Step S5: weigh 85 parts of a main corrosion inhibitor, 8.8 parts of propargyl alcohol, 2.6 parts of sodium dodecylbenzene sulfonate, 55 parts of N,N-dimethylformamide, 40 parts of anhydrous ethanol and 55 parts of deionized water according to weight parts for later use;
[0079] Step S6: Add the main corrosion inhibitor, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 3 hours at a temperature of 65° C. and a stirring rate of 400 r / min to obtain a multifunctional corrosion inhibitor.
[0080] Comparative Example 3:
[0081] This comparative example is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0082] Step S1: 10 mmol benzyl chloride, 40 mmol 4-methylquinoline and 80 mL anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to reflux and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0083] Step S2: 1 g of graphite powder, 30 mL of 98% concentrated sulfuric acid and 0.7 g of sodium nitrate are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 5° C. and a stirring rate of 400 r / min for 50 min, and then 5.5 g of potassium permanganate is added and the mixture is stirred for reaction for 1.5 h at a temperature of 40° C., and then the mixture is stirred for reaction for 1.5 h at a temperature of 100° C. After the reaction is completed, the reaction product is poured into ice water, and then 3 mL of 30% hydrogen peroxide solution is added, and the mixture is allowed to stand for 10 h, and then centrifuged. The precipitate is washed 5 times with a 7% hydrochloric acid solution and distilled water, and then placed in a vacuum drying oven and dried at a temperature of 50° C. for 6 h to obtain graphene oxide;
[0084] Step S3: 1 g of graphene oxide and 35 mL of N,N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 2 h at an ultrasonic frequency of 50 kHz, then 15 g of diethylenetriamine was added and stirred for 15 h at a temperature of 65 ° C and a stirring rate of 400 r / min. After the reaction was completed, the reaction product was cooled to room temperature and then centrifuged. The precipitate was washed with distilled water for 5 times, and then placed in a vacuum drying oven and dried at a temperature of 50 ° C for 4 h to obtain amino-modified graphene oxide;
[0085] Step S4: 1 g of amino-modified graphene oxide, 0.3 g of sodium dodecylbenzene sulfonate and 50 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and a reflux condenser, and ultrasonically treated for 2 h at an ultrasonic frequency of 50 kHz, and then the pH was adjusted to 1 with a 25% hydrochloric acid solution, and then 2 g of aniline and 2.2 g of ammonium persulfate were added and stirred for 10 h at a temperature of 5 ° C and a stirring rate of 400 r / min. After the reaction was completed, the reaction product was centrifuged, and the precipitate was washed 5 times with anhydrous ethanol and distilled water in turn, and then placed in a vacuum drying oven and dried at a temperature of 50 ° C for 8 h to obtain polyaniline-coated modified graphene oxide;
[0086] Step S5: 85 parts of a main corrosion inhibitor, 11.6 parts of polyaniline-coated modified graphene oxide, 8.8 parts of propargyl alcohol, 2.6 parts of sodium dodecylbenzene sulfonate, 55 parts of N,N-dimethylformamide, 40 parts of anhydrous ethanol and 55 parts of deionized water were weighed in parts by weight for later use;
[0087] Step S6: Add the main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 3 hours at a temperature of 65° C. and a stirring rate of 400 r / min to obtain a multifunctional corrosion inhibitor.
[0088] Comparative Example 4:
[0089] This comparative example is a method for preparing a multifunctional corrosion inhibitor, comprising the following steps:
[0090] Step S1: 20 mmol 2-chloro-5-nitrotrifluorotoluene, 10 mmol ethylene glycol, 2 mmol urea and 60 mL dichloromethane were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at 30° C. and a stirring rate of 400 r / min for 25 min, and then the mixture was heated to 85° C. and stirred for 3 h. After the reaction, the reaction product was cooled to room temperature, and then added to distilled water, and then extracted with ethyl acetate for 3 times. The extracts were combined and dried over anhydrous sodium sulfate, and then vacuum filtered. The filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0091] Step S2: 10 mmol of intermediate 1, 0.45 g of 5% palladium carbon and 60 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then hydrogen was introduced to maintain the pressure at 5 MPa and the temperature was raised to 65° C. and continued to stir for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, the filtrate was added to ice water and allowed to stand for precipitation, and then vacuum filtered, the filter cake was placed in a vacuum drying oven, and dried at a temperature of 65° C. for 5 h to obtain intermediate 2;
[0092] Step S3: 10 mmol of intermediate 2, 140 mmol of epichlorohydrin and 1.5 g of tetrabutylammonium bromide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to 80° C. and the stirring reaction was continued for 4 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the excess epichlorohydrin was distilled off under reduced pressure to obtain intermediate 3;
[0093] Step S4: 10 mmol of intermediate 3, 40 mmol of 4-methylquinoline and 80 mL of anhydrous ethanol were added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen was introduced for protection. The mixture was stirred at a temperature of 30° C. and a stirring rate of 400 r / min for 25 min, and then the temperature was raised to reflux and the stirring reaction was continued for 5 h. After the reaction was completed, the reaction product was cooled to room temperature, and then the solvent was removed by rotary evaporation to obtain a main corrosion inhibitor;
[0094] Step S5: 1 g of graphite powder, 30 mL of 98% concentrated sulfuric acid and 0.7 g of sodium nitrate are added to a three-necked flask equipped with a stirrer, a thermometer, an air guide tube and a reflux condenser, and nitrogen is introduced for protection. The mixture is stirred for reaction at a temperature of 5° C. and a stirring rate of 400 r / min for 50 min, and then 5.5 g of potassium permanganate is added and the mixture is stirred for reaction for 1.5 h at a temperature of 40° C., and then the mixture is stirred for reaction for 1.5 h at a temperature of 100° C. After the reaction is completed, the reaction product is poured into ice water, and then 3 mL of 30% hydrogen peroxide solution is added, and the mixture is allowed to stand for 10 h, and then centrifuged. The precipitate is washed 5 times with a 7% hydrochloric acid solution and distilled water, and then placed in a vacuum drying oven and dried at a temperature of 50° C. for 6 h to obtain graphene oxide;
[0095] Step S6: 85 parts of a main corrosion inhibitor, 11.6 parts of graphene oxide, 8.8 parts of propargyl alcohol, 2.6 parts of sodium dodecylbenzene sulfonate, 55 parts of N,N-dimethylformamide, 40 parts of anhydrous ethanol and 55 parts of deionized water were weighed in parts by weight for later use;
[0096] Step S7: Add the main corrosion inhibitor, graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 3 hours at a temperature of 65° C. and a stirring rate of 400 r / min to obtain a multifunctional corrosion inhibitor.
[0097] Performance Test:
[0098] The N80 carbon steel test piece was wiped with acetone, then immersed in anhydrous ethanol for 10 minutes, then taken out and wiped clean, placed in an oven for drying for 6 hours, and after cooling to room temperature, the N80 carbon steel test piece was added to a hydrochloric acid solution with a mass fraction of 20% at a temperature of 120°C and 200°C, and the multifunctional corrosion inhibitors in Examples 1-3 and Comparative Examples 1-4 were added, respectively, and the added amount was 4% of the mass of the hydrochloric acid solution. Then, the corrosion was carried out for 8 hours. After the corrosion experiment was completed and cooled to room temperature, the N80 carbon steel test piece was taken out from the hydrochloric acid solution, and was successively immersed in distilled water and anhydrous ethanol for 10 minutes, then wiped and placed in an oven for drying for 4 hours, and then the performance test was carried out. The test results are shown in the following table:
[0099]
[0100] Among them, the blank case is that the N80 carbon steel test piece is added into the hydrochloric acid solution, and the corrosion test is not performed by adding the multifunctional corrosion inhibitor.
[0101] Referring to the data in the above table, it can be seen that the addition of the main corrosion inhibitor and polyaniline-coated modified graphene oxide can effectively inhibit the high-temperature corrosion effect of the N80 carbon steel specimen, indicating that the multifunctional corrosion inhibitor has excellent high-temperature resistance and corrosion inhibition performance, and when the main corrosion inhibitor and polyaniline-coated modified graphene oxide work synergistically, the comprehensive performance of the multifunctional corrosion inhibitor is the best.
[0102] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0103] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A multifunctional corrosion inhibitor, characterized in that: It includes the following components by weight: 75-85 parts of main corrosion inhibitor, 3.8-11.6 parts of polyaniline-coated modified graphene oxide, 4.2-8.8 parts of propargyl alcohol, 1.2-2.6 parts of sodium dodecylbenzene sulfonate, 45-55 parts of N,N-dimethylformamide, 30-40 parts of anhydrous ethanol and 33-55 parts of deionized water; Wherein, the main corrosion inhibitor is prepared by the following steps: Step A1: 2-chloro-5-nitrotrifluorotoluene, ethylene glycol, urea and dichloromethane are stirred for reaction. After the reaction is completed, the reaction product is cooled and then added to distilled water. The extract is then extracted and dried, and then vacuum filtered and the filtrate is rotary evaporated to obtain intermediate 1; Step A2: Stir and react the intermediate 1, 5% palladium carbon and anhydrous ethanol, then introduce hydrogen and continue stirring the reaction, after the reaction is completed, cool the reaction product, then vacuum filter, add the filtrate into ice water and let it stand for precipitation, then vacuum filter, and dry the filter cake to obtain the intermediate 2; Step A3: stirring the intermediate 2, epichlorohydrin and tetrabutylammonium bromide for reaction, cooling the reaction product after the reaction is completed, and then distilling under reduced pressure to obtain the intermediate 3; Step A4: Stir the intermediate 3, 4-methylquinoline and anhydrous ethanol for reaction. After the reaction is completed, cool the reaction product and then rotary evaporate it to obtain a main corrosion inhibitor.
2. A multifunctional corrosion inhibitor according to claim 1, characterized in that: The usage ratio of the 2-chloro-5-nitrotrifluorotoluene, ethylene glycol, urea and dichloromethane in step A1 is 20 mmol: 10 mmol: 1-2 mmol: 50-60 mL.
3. A multifunctional corrosion inhibitor according to claim 1, characterized in that: The usage ratio of the intermediate 1, 5% palladium carbon and anhydrous ethanol in step A2 is 10 mmol: 0.25-0.45 g: 50-60 mL.
4. A multifunctional corrosion inhibitor according to claim 1, characterized in that: The usage ratio of the intermediate 2, epichlorohydrin and tetrabutylammonium bromide in step A3 is 10 mmol: 120-140 mmol: 0.5-1.5 g.
5. A multifunctional corrosion inhibitor according to claim 1, characterized in that: The usage ratio of the intermediate 3, 4-methylquinoline and anhydrous ethanol in step A4 is 10 mmol:40 mmol:60-80 mL.
6. A multifunctional corrosion inhibitor according to claim 1, characterized in that: The polyaniline-coated modified graphene oxide is prepared by the following steps: Step B1: stirring graphite powder, concentrated sulfuric acid and sodium nitrate for reaction, then adding potassium permanganate and continuing stirring the reaction, pouring the reaction product into ice water after the reaction is completed, then adding hydrogen peroxide solution and letting it stand, then centrifuging, washing and drying the precipitate to obtain graphene oxide; Step B2: subjecting graphene oxide and N,N-dimethylformamide to ultrasonic treatment, and then adding diethylenetriamine to carry out stirring reaction. After the reaction is completed, the reaction product is cooled, and then centrifuged, and the precipitate is washed and dried to obtain amino-modified graphene oxide; Step B3: subjecting the amino-modified graphene oxide, sodium dodecylbenzene sulfonate and deionized water to ultrasonic treatment, and then adjusting the pH, and then adding aniline and ammonium persulfate to stir and react. After the reaction is completed, the reaction product is centrifuged, and the precipitate is washed and dried to obtain polyaniline-coated modified graphene oxide.
7. A multifunctional corrosion inhibitor according to claim 6, characterized in that: The usage ratio of the graphite powder, concentrated sulfuric acid, sodium nitrate, potassium permanganate and hydrogen peroxide solution in step B1 is 1g:20-30mL:0.5-0.7g:4.5-5.5g:2-3mL; the mass fraction of the concentrated sulfuric acid is 98%, and the mass fraction of the hydrogen peroxide solution is 30%.
8. A multifunctional corrosion inhibitor according to claim 6, characterized in that: The usage ratio of the graphene oxide, N,N-dimethylformamide and diethylenetriamine in step B2 is 1g:30-35mL:10-15g.
9. A multifunctional corrosion inhibitor according to claim 6, characterized in that: The usage ratio of the amino-modified graphene oxide, sodium dodecylbenzenesulfonate, deionized water, aniline and ammonium persulfate in step B3 is 1 g: 0.1-0.3 g: 40-50 mL: 1-2 g: 1.8-2.2 g.
10. A method for preparing a multifunctional corrosion inhibitor, characterized in that: The following steps are involved: Step 1: weigh 75-85 parts of main corrosion inhibitor, 3.8-11.6 parts of polyaniline-coated modified graphene oxide, 4.2-8.8 parts of propargyl alcohol, 1.2-2.6 parts of sodium dodecylbenzene sulfonate, 45-55 parts of N,N-dimethylformamide, 30-40 parts of anhydrous ethanol and 33-55 parts of deionized water according to weight parts, and set aside; Step 2: Add the main corrosion inhibitor, polyaniline-coated modified graphene oxide, propargyl alcohol, sodium dodecylbenzene sulfonate, N,N-dimethylformamide, anhydrous ethanol and deionized water into a mixer, stir and react for 2-3 hours at a temperature of 60-65°C and a stirring rate of 300-400r / min to obtain a multifunctional corrosion inhibitor.
Citation Information
Patent Citations
Metal anti-rust agent with excellent vibration reduction performance
CN106978016A
Preparation method of cationic flocculant
CN115259328A
Modified graphene oxide / polyaniline waterborne epoxy resin anticorrosive paint and preparation method thereof
CN116355500A
Solid slow-release anti-corrosion particle for oil well and preparation method thereof
CN116396739A
Acidifying corrosion inhibitor and preparation method thereof
CN118421294A