AgCo-Bi electrocatalyst modified bismuth vanadate photo-anode and preparation method and application thereof
By modifying the AgCo-Bi electrocatalyst on the surface of BiVO4 photoanode, the problems of slow charge mobility and photogenerated electron hole recombination of BiVO4 photoanode are solved, and its photoelectrochemical performance and stability are improved, and more efficient water decomposition performance is achieved.
Patent Information
- Application Number
- CN202411352083.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-06
AI Technical Summary
The charge mobility of BiVO4 photoanode is slow during photoelectric catalysis, and photogenerated electrons and holes are prone to recombination, resulting in low photoelectric conversion efficiency and slow oxidation rate of surface water, causing material corrosion.
The BiVO4 film was modified with AgCo-Bi electrocatalyst. By preparing a bimetallic AgCo-Bi solution and deposition on the BiVO4 surface with heating, the separation efficiency of photogenerated electrons and holes and the surface water oxidation reaction rate were improved.
It significantly improves the charge separation efficiency and surface water oxidation reaction rate of BiVO4, improves the photoelectrochemical water decomposition performance, and enhances the stability and photoelectric conversion efficiency of the material.
Smart Images

Figure CN119082790A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photoelectrode materials, and specifically relates to an AgCo-B i Electrocatalyst modified bismuth vanadate photoanode and preparation method and application thereof. Background Art
[0002] In the context of the increasingly prominent energy crisis in the world, with the growth of global energy demand and the urgent need for renewable energy, hydrogen energy as a clean energy has attracted much attention. Photoelectrochemical (PEC) water splitting hydrogen production technology can use solar energy to split water into hydrogen. Through continuous research and innovation, photoelectrochemical water splitting hydrogen production technology is expected to provide a sustainable solution to energy and environmental problems.
[0003] BiVO4 is an important photoanode material with the potential for widespread application in the field of photoelectrochemistry. It has good light absorption properties in the visible light range, making it an excellent photoanode material for photoelectrochemical reactions. In addition, BiVO4 has high chemical stability and can maintain its structure and properties during photoelectrochemical reactions, thereby improving the durability of photoelectrocatalytic activity. However, BiVO4 has some shortcomings in the photoelectrocatalytic process. The charge mobility of BiVO4 is slow, which is not conducive to the effective separation and transmission of photogenerated carriers. In addition, the photogenerated electrons and holes of BiVO4 are easily recombined inside or on the surface of the material, which reduces its photoelectric conversion efficiency. The water oxidation rate on the surface of bismuth vanadate is slow, and photogenerated holes are easily accumulated on the surface, causing corrosion of the semiconductor itself. Summary of the invention
[0004] Purpose of the invention: The technical problem to be solved by the present invention is to use AgCo-B i Electrocatalysts enhance the efficient separation of photogenerated electrons and holes in BiVO4 and prepare an AgCo-B i Electrocatalyst modified bismuth vanadate photoanode.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A AgCo-B i The preparation method of the electrocatalyst modified bismuth vanadate photoanode comprises the following steps: (1) Preparation of Mo-doped BiVO4 thin films A precursor solution containing Bi, V and Mo elements is prepared, and then the precursor solution is dripped onto the FTO conductive surface, and the precursor solution is formed into a film on the FTO conductive surface by heating the sample, and finally the formed film is calcined to obtain a Mo-doped BiVO4 film; (2) Preparation of bimetallic AgCo-Bi Solution Co(NO3)2·6H2O was added to the boric acid aqueous solution, and after being fully stirred and dissolved, the silver nitrate ethanol solution was added, and the KOH aqueous solution was added under continuous stirring to fully react and obtain the bimetallic AgCo-B i Solution; (3) The bimetallic AgCo-B prepared in step (2) i The solution is heated to 65-75°C, and the BiVO4 film in step (1) is deposited therein while maintaining the temperature, so that the AgCo-B i The electrocatalyst is loaded onto the surface of BiVO4 film to obtain AgCo-B i / BiVO4 photoanode.
[0006] Furthermore, in step (1), in the precursor solution, the molar concentration of Bi element is 0.1-0.3 mol / L; the molar concentration of V is 0.025-0.035 mol / L, the molar concentration of Mo element is 0.005-0.015 mol / L, preferably the molar concentration of Bi element is 0.2 mol / L; the molar concentration of V is 0.03 mol / L, the molar concentration of Mo element is 0.01 mol / L; the molar ratio of Bi, V and Mo is (98-102):(97-100):(1-3), preferably 100:98:2; the solvent for dissolving V and Mo is acetylacetone and / or dimethyl sulfoxide, preferably acetylacetone; the solvent for dissolving Bi is lactic acid and / or glacial acetic acid, preferably lactic acid.
[0007] Furthermore, in step (1), the FTO conductive surface is made of a group of FTO transparent conductive glass, with the conductive surface facing upward.
[0008] Furthermore, in step (1), the precursor solution is 30-40 μL / cm 2 The amount used is dripped onto the FTO conductive surface, preferably 35 μL / cm 2 .
[0009] Furthermore, in step (1), the FTO is preheated to 55-60°C before the precursor solution is added, and the temperature is maintained for 10-15 minutes after the precursor solution is added, and then the FTO is heated to 115-125°C and maintained for 8-15 minutes, preferably 10 minutes.
[0010] Furthermore, in step (1), the calcination temperature is controlled between 470°C and 520°C, the calcination time is 1.5 to 2.5 hours, and after the calcination is completed, the furnace is cooled to room temperature, preferably 500°C for 2 hours.
[0011] Furthermore, in step (2), the concentration of the boric acid aqueous solution is 0.75-0.85 mol / L; Co(NO3)2·6H2O and the boric acid aqueous solution are mixed at a mass volume ratio of 0.00055-0.0006 g / ml; the concentration of the silver nitrate ethanol solution is 0.045-0.055 mol / L; the concentration of the KOH aqueous solution is 0.35-0.45 mol / L; the volume ratio of the boric acid aqueous solution, the silver nitrate ethanol solution, and the KOH aqueous solution is (71-80): (1.34-1.63): (67-86). Preferably 75:1.47:75.
[0012] Furthermore, in step (2), the BiVO4 film is formed on a bimetallic AgCo-B i The deposition time in the solution is 10 to 90 seconds, preferably 45 seconds.
[0013] Furthermore, the AgCo-B prepared by the above preparation method i The electrocatalyst-modified bismuth vanadate photoanode is also within the protection scope of the present invention.
[0014] Furthermore, the present invention also claims the above-mentioned AgCo-B i Application of electrocatalyst modified bismuth vanadate photoanode for photoelectrochemical water splitting to decompose water into hydrogen using solar energy. Beneficial Effects
[0015] (1) Ag and Co borate compounds were loaded onto the surface of BiVO4 photoanode by water bath heating method to obtain BiVO4 composite photoanode modified with Ag and Co bimetallic borate compounds. i Electrocatalysts enhance the effective separation of photogenerated electrons and holes in BiVO4, and can be used to improve the charge separation efficiency and surface water oxidation reaction rate of BiVO4, thereby effectively improving the photoelectrochemical water splitting performance of BiVO4.
[0016] (2) Adding Mo to the precursor solution for preparing BiVO4 thin film can significantly improve its conductive properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0018] Figure 1 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / BiVO4 photoanode XRD pattern.
[0019] Figure 2 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / BiVO4 photoanode; a is the SEM image of BiVO4, b is the SEM image of AgCo-B i SEM image of / BiVO4 photoanode, c is Ag-B i SEM image of / BiVO4 photoanode, d is Co-B i SEM image of / BiVO4 photoanode.
[0020] Figure 3 AgCo-B i TEM image of / BiVO4 photoanode; where a is AgCo-B i TEM image of / BiVO4 photoanode, b is HR-TEM image, and the rest are AgCo-B i HAADF-EDS image of / BiVO4 photoanode.
[0021] Figure 4 The full spectrum test diagram of XPS for each photoanode; a is BiVO4 and AgCo-B i / BiVO4 photoanode XPS full spectrum test chart, b is C 1s, c is Bi 4f, d is V 2p, e is O 1s, f is Mo 3d, g is Ag 3d, h is B 1s, and i is the XPS spectrum of Co2p.
[0022] Figure 5 is the UV-visible light absorption spectrum of each photoanode; where a is BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / BiVO4 photoanode UV-visible absorption spectrum, b is the tauc conversion diagram.
[0023] Figure 6 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i OCP curve of / BiVO4 photoanode.
[0024] Figure 7 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-Bi Impedance analysis diagram of / BiVO4 photoanode; wherein, a is the impedance diagram at a voltage of 0.6V, b is the impedance diagram at a voltage of 0.55V, c is the impedance diagram at a voltage of 0.5V, and d is the impedance diagram at a voltage of 0.45V.
[0025] Figure 8 a is AgCo-B i / BiVO4 photoanode performance diagram of photoelectrochemical water splitting under different loading time, b is BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i Performance diagram of photoelectrochemical water splitting of / BiVO4 photoanode when the loading time is 45s.
[0026] Fig. 9 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i Stability diagram of the / BiVO4 photoanode. DETAILED DESCRIPTION
[0027] The present invention can be better understood with reference to the following examples. Example 1
[0028] Step 1: Prepare BiVO4 thin film by drop coating. Prepare BiVO4 precursor solution by mixing Bi, V and Mo solutions in a volume ratio of 75:490:30 (Mo is added to improve its conductivity). Use a pipette to draw 35 μL of precursor solution and drop it onto the cleaned FTO (1*2 cm) transparent conductive glass (half of the FTO is covered with heat-resistant tape, and 1 cm is exposed). 2 FTO was first heated on a heating table (60 °C, 10 min), then the temperature was raised to 120 °C and heated for 10 min. After the initial film was formed, it was placed in a calcination furnace and calcined (500 °C, 2 h). After the calcination furnace cooled to room temperature, the sample was taken out to obtain the BiVO4 sample.
[0029] Step 2: Preparation of bimetallic AgCo-B iSolution. First, weigh 0.0849 g of silver nitrate and put it into a screw-mouth glass bottle. First, add 400 microliters of deionized water. After the silver nitrate particles are completely dissolved, add 9.6 ml of ethanol to obtain a 0.05 mol / L silver nitrate ethanol solution. Weigh 3.71 g of boric acid and add it to 75 ml of deionized water. Then weigh 0.043 g of Co(NO3)2·6H2O and pour it into a beaker containing the prepared boric acid solution. Place the beaker on a magnetic stirrer and put a clean rotor in it to stir for 5 to 10 min until it dissolves. Then use a pipette to draw 1470 μL of the ethanol solution of silver nitrate and slowly drip it into the prepared boric acid solution. Continue stirring, then dissolve 1.69 g of KOH in a beaker containing 75 ml of deionized water. After the potassium hydroxide is completely dissolved, slowly pour it into the previously prepared solution to obtain AgCo-B. i Solution.
[0030] Step 3: BiVO4 obtained in step 1 is loaded by chemical bath deposition, and the AgCo-B prepared in step 2 is loaded i The solution was placed in the center of the water bath and heated. When the temperature rose to 70 °C, the BiVO4 prepared in step 1 was added. Then, AgCo-B was obtained by changing the deposition time. i / BiVO4 photoanode. In this experiment, the bimetallic AgCo-B i The loading time in the solution was 45 s. Example 2
[0031] The difference from Example 1 is that in step 3, BiVO4 is formed on the bimetallic AgCo-B i The loading time in the solution was 90 s. Example 3
[0032] The difference from Example 1 is that in step 3, BiVO4 is formed on the bimetallic AgCo-B i The loading time in the solution was 10 s. Comparative Example 1
[0033] The difference from Example 1 is: Step 2: Prepare single metal Ag-B i Solution, first weigh 3.71 g of boric acid and add it to a beaker filled with 75 ml of deionized water and place a clean rotor in it, then move the beaker to a magnetic stirrer, after the boric acid solution is prepared, use a pipette to draw 1470 μL of silver nitrate ethanol solution, and continue stirring with a magnetic stirrer for 5-10 min, then dissolve 1.69 g of KOH in a beaker filled with 75 ml of deionized water, and after the potassium hydroxide is dissolved, slowly pour it into the previously prepared solution to obtain the single metal Ag-B i Solution.
[0034] Step 3: BiVO4 obtained in step 1 is loaded by chemical bath deposition, and the Ag-B prepared in step 2 is added to the i The solution was placed in the center of the water bath and heated. When the temperature rose to 70 °C, the BiVO4 prepared in step 1 was added. Then, the Ag-B i / BiVO4 photoanode. In this experiment, Ag-B i The time of liquid loading is 45s. Comparative Example 2
[0035] The difference from Example 1 is: Step 2: Prepare single metal Co-B i Solution, first weigh 3.71 g of boric acid and add it to a beaker filled with 75 ml of deionized water and place a clean rotor in it, then move the beaker to a magnetic stirrer, wait for the boric acid solution to be prepared, weigh 0.043 g of Co(NO3)2·6H2O and pour it into the prepared boric acid solution, continue stirring with a magnetic stirrer for 5-10 min, then dissolve 1.69 g of KOH in a beaker filled with 75 ml of deionized water, wait for the potassium hydroxide to dissolve, slowly pour it into the previously prepared solution, and the monometallic Co-B i of solution.
[0036] Step 3: The BiVO4 obtained in step 1 is loaded by chemical bath deposition, and the Co-B prepared in step 2 is loaded i The solution was placed in the center of the water bath and heated. When the temperature rose to 70 °C, the BiVO4 prepared in step 1 was added. Then, the Co-B i / BiVO4 photoanode. This experiment selected single metal solution Co-B i The time of liquid loading is 45s. Results Analysis
[0037] Figure 1 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / XRD pattern of BiVO4 photoanode. From the XRD spectrum, it can be seen that BiVO4 after loading with Ag and Co metal ions does not produce new diffraction peaks, and the physical phase difference is not big, so the loading does not change the crystal structure of BiVO4.
[0038] Figure 2 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / SEM image of BiVO4 photoanode. After loading with AgCo, the basic structure of BiVO4 did not change significantly, the pores on the surface became smaller, and Ag and Co particles could be clearly seen, indicating that AgCo was successfully loaded on the BiVO4 surface.
[0039] Figure 3 AgCo-B i TEM and HR-TEM images of / BiVO4 photoanode. The results show that BiVO4 and AgCo-B i Tightly bonded. AgCo-B i EDS elemental analysis of the / BiVO4 photoanode proved that Ag and Co plasma were successfully deposited on BiVO4.
[0040] Figure 4 In the figure, a is BiVO4 and AgCo-B i / BiVO4 photoanode XPS full spectrum test chart, BiVO4 and AgCo-B i / BiVO4 contains carbon, oxygen, bismuth, molybdenum, and vanadium. In addition, AgCo-B i / BiVO4 contains silver, cobalt and boron. Figures b, c, d, e and f are the XPS spectra of C1s, Bi 4f, V 2p, O 1s and Mo 3d respectively. In figure c, we can see that the two characteristic peaks of BiVO4 are Bi 4f 7 / 2 158.8 eV, Bi 4f 5 / 2 164.1 eV, the characteristic peak after loading AgCo remains almost unchanged, indicating that both samples contain Bi 3+ Figure e shows that the position of the O 1s peak changes after loading AgCo. Figures g, h, and i show the XPS spectra of Ag 3d, B 1s, and Co 2p, from which it can be seen that the chemical bath deposition method successfully loads Ag and Co plasma onto BiVO4.
[0041] Figure 5 In the figure, a is BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i The UV-visible absorption spectra of the AgCo-B photoanode are shown in Figure 2. In general, the absorbance trends of the four materials are similar. When the wavelength is below 280 nm, the absorbance increases, and when the wavelength is above 280 nm, the absorbance decreases. The absorbance of BiVO4 loaded with metal ions is significantly improved compared with that of pure BiVO4. i / BiVO4>Ag-B i / BiVO4>Co-B i / BiVO4, in the figure b is BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i The tauc conversion diagram of the / BiVO4 photoanode. The bandgap width of these four samples is 2.31 eV, which shows that BiVO4 is a material with a suitable bandgap and excellent visible light response.
[0042] Figure 6 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / BiVO4 photoanode OCP curve. It can be seen from the figure that the OCP difference of BiVO4 after loading is AgCo-B i / BiVO4>Ag-B i / BiVO4>Co-B i / BiVO4, so the sample loaded with AgCo bimetallic ions has higher electrochemical activity and greater charge transfer efficiency.
[0043] Figure 7 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i Electrochemical impedance spectroscopy of the AgCo-B / BiVO4 photoanode. i / BiVO4 photoanode has the smallest radius, so the charge transfer rate on the electrocatalyst surface is the highest and the electrochemical reaction proceeds fastest, followed by BiVO4 loaded with single metal Ag ions, and then that loaded with single metal Co ions. This performance data is consistent with the order of photocurrent density.
[0044] Figure 8 In the figure, a is AgCo-B i / BiVO4 photoanode photoelectrochemical water splitting performance diagram at different loading times. It can be seen from the figure that the photocurrent density is the highest at 45s. b is BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / BiVO4 photoanode photoelectrochemical water splitting performance diagram at 45s. It can be seen from the figure that when the loading time is 45s, the performance of AgCo dual gold ion BiVO4 is significantly higher than that of single metal. The photocurrent density loaded with bimetallic AgCo ions is nearly 1.66 times higher than that loaded with single metal Ag ions, and nearly 3.07 times higher than that loaded with single metal Co ions.
[0045] Fig. 9 BiVO4, Ag-B i / BiVO4、Co-B i / BiVO4、AgCo-B i / BiVO4 photoanode stability diagram. It can be seen from the figure that the PEC stability after BiVO4 loading is better than that before loading.
[0046] The present invention provides an AgCo-B i The electrocatalyst-modified bismuth vanadate photoanode and its preparation method and application ideas and methods, there are many methods and ways to implement the technical solution, the above is only a preferred embodiment of the present invention, it should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made, and these improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A AgCo-B i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: The steps include: (1) Preparation of Mo-doped BiVO4 thin films A precursor solution containing Bi, V and Mo elements is prepared, and then the precursor solution is dripped onto the FTO conductive surface, and the sample is heated so that the precursor solution forms a film on the FTO conductive surface, and finally the formed film is calcined to obtain a Mo-doped BiVO4 film; (2) Preparation of bimetallic AgCo-B i Solution Co(NO3)2·6H2O was added to the boric acid aqueous solution, and after being fully stirred and dissolved, the silver nitrate ethanol solution was added, and the KOH aqueous solution was added under continuous stirring to fully react and obtain the bimetallic AgCo-B i Solution; (3) The bimetallic AgCo-B prepared in step (2) i The solution is heated to 65-75 °C, and the BiVO4 film in step (1) is deposited therein while maintaining the temperature, so that the AgCo-B i The electrocatalyst is loaded on the surface of the BiVO4 film.
2. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (1), in the precursor solution, the molar concentration of Bi element is 0.1-0.3 mol / L; the molar concentration of V is 0.025-0.035 mol / L, and the molar concentration of Mo element is 0.005-0.015 mol / L; the molar ratio of Bi, V and Mo is (98-102):(97-100):(1-3); the solvent for dissolving V and Mo is acetylacetone and / or dimethyl sulfoxide, and the solvent for dissolving Bi is lactic acid and / or glacial acetic acid.
3. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (1), the FTO conductive surface is a surface of the FTO transparent conductive glass, and the conductive surface faces upward.
4. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (1), the precursor solution is 30-40 μL / cm 2 Add the amount of use dropwise onto the conductive surface.
5. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (1), the FTO conductive surface is preheated to 55-60°C before the precursor solution is added, and maintained for 10-15 minutes after the precursor solution is added, and then the sample is heated to 115-125°C and maintained for 8-15 minutes.
6. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (1), the calcination temperature is controlled between 470 and 520°C, the calcination time is 1.5 to 2.5 hours, and after the calcination is completed, the furnace is cooled to room temperature.
7. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (2), the concentration of the boric acid aqueous solution is 0.75-0.85 mol / L; Co(NO3)2·6H2O and the boric acid aqueous solution are mixed at a mass volume ratio of 0.00055-0.0006 g / ml; the concentration of the silver nitrate ethanol solution is 0.045-0.055 mol / L; the concentration of the KOH aqueous solution is 0.35-0.45 mol / L; the volume ratio of the boric acid aqueous solution, the silver nitrate ethanol solution and the KOH aqueous solution is (71-80):(1.34-1.63):(67-86).
8. The AgCo-B according to claim 1 i The method for preparing a bismuth vanadate photoanode modified with an electrocatalyst is characterized in that: In step (2), the BiVO4 film is formed on a bimetallic AgCo-B i The deposition time in the solution is 10~90 s.
9. The AgCo-B prepared by the preparation method according to any one of claims 1 to 8 i Electrocatalyst modified bismuth vanadate photoanode.
10. The AgCo-B according to claim 9 i Application of electrocatalyst modified bismuth vanadate photoanode for photoelectrochemical water splitting.