Rare earth biological protein fiber, and preparation method and application thereof
Through the combination of rare earth nanoparticles and silk fibroin, NaNdF4 and silk fibroin modified by Teng's blue or Brussian blue were used to prepare efficient rare earth biological protein fibers, which solved the poor mechanical properties and low photothermal efficiency of existing photothermal fibers. The problem of high efficiency photothermal conversion and high mechanical strength under extreme conditions.
Patent Information
- Application Number
- CN202411364814.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-27
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of biotechnology, and in particular to rare earth biological protein fiber, a preparation method and application thereof. Background Art
[0002] Fiber materials play a vital role in the field of national economy and people's livelihood. At a time when resources and energy are becoming increasingly scarce and extreme climates are frequent, biofibers with high mechanical properties and thermal management functions represent the future development trend and are of great significance to protecting personal life and health and national equipment safety.
[0003] At present, photothermal fibers can be divided into active and passive thermal regulation. Passive thermal regulation refers to thermal regulation by regulating the body's own heat production and heat dissipation without relying on external energy. Active thermal regulation is to assist in heating or cooling the human body with the input of external energy. However, the above scenarios still require electric energy drive and are difficult to apply under extreme conditions. At present, there are still few studies on the direct use of solar energy to achieve efficient photothermal conversion fiber materials and equipment thermal storage applications. For example, photothermal fibers are prepared and woven using materials such as silk fibroin and polydopamine (PDA) composite fibers and carbon fiber @MXene. However, the mechanical properties of the photothermal fibers used in these studies are poor, less than 200 MPa, and the photothermal efficiency is only about 30%. Therefore, the development of high-performance rare earth biofibers with wide-spectrum photothermal conversion functions can provide new material support for the preparation of thermal storage equipment under extreme conditions. Summary of the invention
[0004] In view of this, the technical problem to be solved by the present invention is to provide rare earth bioprotein fiber, a preparation method and application thereof.
[0005] The present invention provides biological protein fibers, the raw materials of which include rare earth nanoparticles and silk fibroin;
[0006] The rare earth nanoparticles are NaNdF4 modified with Teng's blue or Bruce's blue;
[0007] The mass ratio of the rare earth photothermal nanoparticles to the silk fibroin is (0.1-1.5): (10-20);
[0008] In the present invention, the rare earth photothermal nanoparticles are NaNdF4 modified with Teng's blue or Bruce's blue; Fe 2+ With [Fe(CN)6] 4- Reaction, generating a dark blue precipitate, which is Prussian blue; Fe 2+ With [Fe(CN)6] 3-The two products show similar colors (blue) and contain exactly the same chemical elements and chemical formulas. The properties of the two products are the same or basically the same as those of the two products in the determination of X-ray, magnetic susceptibility, photoelectron spectrum and Mössbauer spectrum. In the present invention, the two products can be replaced with each other. In the actual reaction, potassium ferrocyanide K4Fe(CN)6 contains ferrocyanide complex ions [Fe(CN)6] 4- , and Fe 2+ The blue product obtained by the reaction is Prussian blue; potassium ferrocyanide K3Fe(CN)6 contains ferrocyanide complex ion [Fe(CN)6] 3− , and Fe 2+ The blue product obtained by the reaction is Teng's blue; in a specific embodiment of the present invention, Teng's blue is obtained by using potassium ferrocyanide for the reaction.
[0009] Furthermore, the mass ratio of the rare earth nanoparticles to silk fibroin is (0.1-1.5):(10-20); furthermore, (0.5-1.5):15.
[0010] In the present invention, the mass ratio of rare earth nanoparticles to silk fibroin is (0.1~1.5):(10~20); in a specific embodiment of the present invention, the mass ratio of rare earth nanoparticles to silk fibroin can be 0.5:15; it can also be 1:15; it can also be 1.5:15; experimental results show that when the mass ratio of rare earth nanoparticles to silk fibroin is 1:15, it has high photothermal efficiency and high mechanical strength, wherein the photothermal efficiency can reach 56%, and the mechanical strength can reach 512±27 MPa.
[0011] The rare earth nanoparticles have a particle size of 180nm to 220nm and have a cluster-like morphology;
[0012] The rare earth nanoparticles are NaNdF4 modified with Teng's blue.
[0013] In the present invention, the silk fibroin can be homemade or purchased, and the present invention is not limited to this; further, in a specific embodiment of the present invention, the silk fibroin is obtained by degumming silk, which is a conventional technical means adopted by those skilled in the art; further, specifically, the preparation steps of the silk fibroin are: chopping tussah pupae, immersing them in a 0.5wt% sodium carbonate solution at a ratio of 10g / L, boiling for 30 minutes, then washing and drying to obtain degummed silk, which is the silk fibroin described in the present invention.
[0014] In the present invention, the nanoparticles can be obtained by directly doping the nanoparticles obtained by modifying with Teng's blue and silk fibroin to obtain the photothermal protein fiber of the present invention, or the unmodified NaNdF4 can be modified with Teng's blue in situ during the spinning process to obtain the photothermal protein fiber of the present invention, and the present invention is not limited to this. The test results of the present invention show that the performance of the photothermal protein fiber prepared by the direct doping method is slightly better than that of the in situ modification method.
[0015] The present invention provides a method for preparing the biological protein fiber, which comprises the following steps:
[0016] The rare earth nanoparticles and silk fibroin are wet-spun in the presence of a cosolvent and an organic acid to obtain the bioprotein fiber.
[0017] The co-solvents include CaCl2 and LaCl3.
[0018] The mass concentration ratio of the rare earth nanoparticles, silk fibroin, CaCl2 and LaCl3 is (0.1~1.5):(10~20):2:2; more specifically, in an embodiment of the present invention, the mass concentration ratio of the rare earth nanoparticles, silk fibroin, CaCl2 and LaCl3 is (0.1~1.5):15:2:2; more specifically, the mass concentration ratio of the rare earth nanoparticles, silk fibroin, CaCl2 and LaCl3 is 0.5:15:2:2 or 1:15:2:2 or 1.5:15:2:2; experimental results show that when the mass ratio of rare earth nanoparticles and silk fibroin is 1:15, it has high photothermal efficiency and high mechanical strength at the same time, wherein the photothermal efficiency can reach 56%, and the mechanical strength can reach 512±27 MPa.
[0019] The organic acid is formic acid.
[0020] The extrusion speed of the wet spinning is 10-40 μL / min;
[0021] The coagulation liquid of the wet spinning is a mixture of ethanol and water, wherein the ethanol content is 30vt% to 70vt%.
[0022] In the present invention, the role of CaCl2 in the dissolution and regeneration process of silk fibroin can help the silk fibroin dissolve in a specific solvent to form a uniform solution, which is very important for the subsequent spinning step; LaCl3 and CaCl2 work synergistically to promote the dissolution of silk fibroin in the solvent, and may also affect the molecular structure and arrangement of silk fibroin, thereby affecting the performance of the final fiber; formic acid, as an organic acid, may help adjust the pH value of the solution, thereby affecting the solubility and molecular structure of silk fibroin, so CaCl2, LaCl3 and formic acid work together in the process of silk fibroin spinning to affect the spinning effect.
[0023] The wet spinning process further includes a stretching step, wherein the stretched length is 0% to 600% of the original filament length.
[0024] Furthermore, in the present invention, the method for preparing the rare earth nanoparticles comprises the following steps:
[0025] Step 1, mixing neodymium salt in a mixed solvent of oleic acid and octadecene, and then reacting with a sodium source and a fluorine source for a first reaction and then precipitating to obtain NaNdF4;
[0026] Step 2, mixing the NaNdF4 and NOBF4 and centrifuging to collect the precipitate, and modifying the precipitate with citric acid to obtain NaNdF4@CA;
[0027] Step 3: The NaNdF4@CA reacts with cyanide in the presence of FeSO4 and citric acid to obtain the rare earth nanoparticles.
[0028] Furthermore,
[0029] In step 1,
[0030] The neodymium salt includes at least one of NdCl3, Nd(NO3)3, Nd(CH3CO2)3, Nd(TFA)3 or Nd(ACAC)3; specifically, the neodymium salt is NdCl3;
[0031] The sodium source includes at least one of sodium oleate, NaF, NaTFA or NaOA; specifically, the sodium source is sodium oleate;
[0032] The fluorine source includes any one of NH4F or NaF; specifically, the fluorine source is NH4F;
[0033] In the mixed solvent of oleic acid and octadecene, the volume ratio of oleic acid to octadecene is 3:7;
[0034] The molar ratio of the neodymium salt, the sodium source and the fluorine source is: (0.5-1.5): (3-4): (1-1.5); specifically 1:3.3:1.25; in a specific embodiment of the present invention, NdCl3 is dissolved in oleic acid and octadecene to a final concentration of 1 mmol, and then NH4F and sodium oleate are added to a concentration of 3.3 mmol and a concentration of 1.25 mmol of NH4F and sodium oleate after addition.
[0035] The conditions of the first reaction are: heating to 110°C in vacuum and then heating to 310°C under N2 protection for 40 min;
[0036] The precipitating reagent is anhydrous ethanol;
[0037] The method further comprises a first washing step after the precipitation; the reagent for the first washing comprises ethanol and / or cyclohexane, and specifically, washing is performed using ethanol and cyclohexane in sequence.
[0038] In step 2,
[0039] The mass ratio of NaNdF4 to NOBF4 is (25-30):(3-8). Specifically, in a specific embodiment of the present invention, the mass ratio of NaNdF4 to NOBF4 is 27.273:(3.6-7.27). To 10 mL of n-hexane solution containing 300 mg NaNdF4, 1 mL of N,N-dimethylformamide (DMF) solution containing 40-80 mg / mL NOBF4 is added. More specifically, in a specific embodiment of the present invention, the mass concentration ratio of NaNdF4 to NOBF4 is 27.273:5.455. To 10 mL of n-hexane solution containing 300 mg NaNdF4, 1 mL of N,N-dimethylformamide (DMF) solution containing 60 mg / mL NOBF4 is added.
[0040] The citric acid modification condition is to immerse in a citric acid solution and ultrasonicate for 30 minutes;
[0041] The concentration of the citric acid solution is 50% to 64.3%. In a specific embodiment of the present invention, it is a saturated citric acid solution with a specific concentration of 64.3%.
[0042] In step 3,
[0043] The mass ratio of the NaNdF4@CA, FeSO4, citric acid and K3Fe(CN)6 is (0.01~0.1):(3~4):(4~5.5):(7.5~9); in a specific embodiment of the present invention, the mass ratio of the NaNdF4@CA, FeSO4, citric acid and K3Fe(CN)6 is 0.06:3.8:4.803:8.225; 1 mL of 60 mg / L NaNdF4@CA solution is added to 50 mL of water, 5 mL of FeSO4 and CA aqueous solution is added, and then 5 mL of K3Fe(CN)6 (potassium ferrocyanide) aqueous solution with the same concentration as FeSO4 is added. The concentrations of FeSO4 and CA before addition are preferably 5 mM FeSO4 and 0.09M CA.
[0044] The cyanide is potassium ferrocyanide and / or potassium ferrocyanide; if the cyanide is potassium ferrocyanide, the rare earth nanoparticles are NaNdF4 modified with Teng's blue; if the cyanide is potassium ferrocyanide, the rare earth nanoparticles are NaNdF4 modified with Bruce's blue; in a specific embodiment of the present invention, the cyanide is potassium ferrocyanide.
[0045] After the reaction with cyanide, the method further includes the steps of centrifugation and washing, wherein the washing solution is a mixture of water and acetone, wherein the content of acetone is 30vt% to 70vt%, specifically, the content of acetone is 50vt%.
[0046] In the present invention, the mixed solution can be extruded into a coagulation solution for spinning and then post-stretched, and the stretching length is 0% to 600% of the original filament length to obtain the bioprotein fiber of the present invention.
[0047] The present invention optimizes the preparation method of the biological protein fiber. In a specific embodiment of the present invention, the biological protein fiber is prepared by an in-situ modification method and a direct doping method. Experimental results show that the biological protein fiber obtained by the direct doping method has higher strength, better toughness and modulus, and better photothermal efficiency.
[0048] In other specific embodiments of the present invention, the mass ratio of silk fibroin to rare earth nanoparticles is optimized. In specific embodiments of the present invention, the mass ratio of silk fibroin to rare earth nanoparticles can be 15:0.5; 15:1; or 15:1.5. Experimental results show that when the mass ratio of silk fibroin to rare earth nanoparticles is 15:1, the photothermal efficiency is the highest and the mechanical strength is high, wherein the photothermal efficiency can reach 56% and the mechanical strength can reach 512±27MPa.
[0049] The present invention mainly utilizes silk fibroin structure assembly for fiber forming. Usually, the introduction of inorganic nanoparticles (the rare earth nanoparticles of the present invention are inorganic nanoparticles) will affect the protein structure assembly, resulting in reduced performance, especially in the in-situ synthesis process. The present invention achieves the synergy of mechanical and photothermal performance by regulating the process; in the specific embodiment of the present invention, the preparation method of the biological protein fiber is adjusted, and the preparation method of the corresponding rare earth nanoparticles is also adaptively changed; in addition, the present invention also adjusts the doping concentration of rare earth nanoparticles and silk fibroin to obtain the biological protein fiber of the present invention with both photothermal and mechanical properties.
[0050] The present invention provides a photothermal nanocomposite material, which comprises at least one of the bioprotein fibers described in the present invention and / or the bioprotein fibers prepared by the preparation method described in the present invention and a matrix thereof.
[0051] Furthermore, the substrate includes cloth, resin, rubber, ceramic and / or metal.
[0052] In the present invention, the bioprotein fiber has the characteristics of excellent mechanical stability and easy regeneration and processing, and becomes a preferred hot material for wearable products. At the same time, the bioprotein fiber of the present invention can be used in the biomedical field for the development of bionic structures, such as membranes, gels, and scaffolds. The bioprotein fiber of the present invention can also be processed into thin films, gels and other materials, and can be applied to optoelectronic devices and bioimaging through modification and functionalization.
[0053] In the present invention, the photothermal nanocomposite material includes but is not limited to textile materials, equipment, cables and / or coatings.
[0054] The present invention provides at least one application of the following A) to C) in the field of electrical and / or optical conductors, the field of smart wearables and / or the field of medical bionics:
[0055] A), the biological protein fiber of the present invention;
[0056] B), biological protein fiber obtained by the preparation method of the present invention;
[0057] C) The photothermal nanocomposite material of the present invention.
[0058] Specifically, in a specific embodiment of the present invention, it is used in the field of smart wearables for bioheat storage.
[0059] The present invention uses rare earth nanoparticles and silk fibroin as raw materials and utilizes a direct doping method to synthesize the bioprotein fiber described in the present invention. Experimental results show that the bioprotein fiber described in the present invention has both high photothermal efficiency and mechanical properties, providing a new strategy for the development of new high-performance photothermal fibers, and can be widely used in the preparation of special outdoor thermal insulation equipment for extreme environments.
[0060] The method for heat preservation and / or heat conduction is to use at least one of the following a) to c) to perform heat preservation and / or heat conduction:
[0061] a), the biological protein fiber of the present invention;
[0062] b) Bioprotein fiber obtained by the preparation method of the present invention;
[0063] c) The photothermal nanocomposite material of the present invention.
[0064] The present invention uses rare earth nanoparticles and silk fibroin as raw materials and utilizes a direct doping method to synthesize the bioprotein fiber described in the present invention. Experimental results show that the bioprotein fiber described in the present invention has both high photothermal efficiency and mechanical properties, providing a new strategy for the development of new high-performance photothermal fibers, and can be widely used in the preparation of special outdoor thermal insulation equipment for extreme environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 TEM image of the rare earth photothermal nanoparticles obtained in Example 1, scale: 50 nm;
[0066] Figure 2 2 is a graph showing the tensile mechanical properties of the fiber obtained by post-stretching treatment in Example 2;
[0067] Figure 3 1 is a graph showing the tensile mechanical properties of the fiber obtained by post-stretching treatment in Example 3;
[0068] Figure 4 2 is a graph showing the light and heat performance of the fiber obtained by post-drawing treatment in Example 2;
[0069] Figure 5 The photothermal performance curve of the fiber obtained by post-drawing treatment in Example 3 is shown. DETAILED DESCRIPTION
[0070] The present invention provides rare earth bioprotein fibers, preparation methods and applications thereof. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve the above. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0071] In the present invention, the preparation steps of silk fibroin are as follows: tussah pupae are cut into pieces, immersed in a 0.5 wt% sodium carbonate solution at a ratio of 10 g / L, boiled for 30 minutes, washed and dried, and degummed silk is obtained.
[0072] The biological protein fiber described in the present invention is a rare earth protein fiber with both mechanical properties and photothermal properties. The present invention uses the special light response properties of rare earth elements to achieve the engineering preparation of rare earth high-strength and high-toughness biological fibers with photothermal functions. The fiber can achieve efficient photothermal conversion under sunlight and promote the high-value application of rare earth resources.
[0073] At the same time, the Prussian blue or Teng's blue coated NaNdF4 photothermal molecules and fiber composite methods were innovated, and the in-situ photothermal molecular synthesis technology was innovatively developed. Usually, the introduction of inorganic nanoparticles will affect the assembly of protein structures, resulting in reduced performance, especially in the in-situ synthesis process. By regulating the process, the synergy of mechanical and photothermal properties was achieved.
[0074] Traditional inorganic composite strategies often greatly reduce the mechanical properties of fibers. The strategy provided by the present invention can maintain the mechanical properties of fibers while having excellent photothermal conversion characteristics. The present invention effectively assembles rare earth photothermal nanoparticles with protein / biomacromolecule systems to achieve compatibility between mechanical properties and photothermal efficiency, thereby obtaining photothermal protein fiber materials with high mechanical properties and high photothermal efficiency; the photothermal protein fiber has excellent mechanical properties, wearing comfort, and degradability, and has important application value in the field of special clothing, providing a new strategy for the development of a new generation of rare earth biomaterials.
[0075] The test materials used in the present invention are all common commercial products and can be purchased on the market. The present invention is further described below in conjunction with the embodiments:
[0076] Example 1 Preparation of rare earth photothermal nanoparticles
[0077] Dissolve 1mmol NdCl3 in 20mL oleic acid and octadecene, oleic acid / octadecene is 3 / 7 (v / v), add NH4F and sodium oleate under stirring, preferably 3.3mmol and 1.25mmol respectively. Evacuate and raise the temperature to 110℃, then heat to 310℃ under N2 protection and keep for 40min, cool to room temperature and add ethanol for precipitation, centrifuge, and wash with ethanol and cyclohexane in turn, the product is dispersed in cyclohexane or n-hexane;
[0078] Add 1 mL of N,N-dimethylformamide (DMF) solution containing NOBF4 to 10 mL of n-hexane solution containing 300 mg of NaNdF4, preferably 60 mg / mL of NOBF4. Centrifuge and add 5 mL of saturated citric acid CA solution (the concentration of the citric acid solution is 64.3%) to the precipitate, and ultrasonicate for 30 min to obtain NaNdF4@CA nanoparticles;
[0079] Take 1mL of 60 mg / L NaNdF4@CA solution and add it to 50mL of water, add 5mL of FeSO4 and CA aqueous solution, and then add 5mL of K3Fe(CN)6 (potassium ferrocyanide) aqueous solution with the same concentration as FeSO4. The concentration of FeSO4 and CA is preferably 5mM FeSO4 and 0.09M CA. Centrifuge and wash with a mixture of water / acetone (acetone content is 50vt%), and the product is dispersed in water. The nanoparticles were analyzed by transmission electron microscopy and showed a clustered morphology with a size of about 200nm and uniform distribution, as shown in Figure 2. Figure 1 As shown; the centrifugal speed of the present invention is 6000rpm.
[0080] Example 2 Preparation of 0.5% NaNdF4@TB rare earth photothermal biofiber by direct doping
[0081] Prepare a formic acid solution of silk fibroin and NaNdF4@TB. The concentration of silk fibroin is preferably 15wt%, and the concentration of NaNdF4@TB is preferably 0.5wt%. The silk fibroin is dissolved in a spinning solution, and the spinning solution contains CaCl2 and LaCl3, and their concentrations are preferably 2wt%. The protein solution is extruded into a coagulation bath for wet spinning, and the fibers are collected. The extrusion speed is preferably 15μL / min. The coagulation bath is a mixed solution of ethanol and water, and the proportion of ethanol is preferably 50%. A high-performance rare earth photothermal biofiber is obtained. The collected fibers are post-stretched to obtain rare earth photothermal biofibers with good mechanical properties, wherein the post-stretching degree is preferably 600% of the original fiber length.
[0082] Example 3 Preparation of 1% NaNdF4@TB rare earth photothermal biofiber by direct doping
[0083] Prepare a formic acid solution of silk fibroin and NaNdF4@TB. The concentration of silk fibroin is preferably 15wt%, the concentration of NaNdF4@TB is preferably 1wt%, and CaCl2 and LaCl3 are dissolved in the spinning solution, and their concentrations are preferably 2wt%. The protein solution is extruded into a coagulation bath for wet spinning, and the fibers are collected. The extrusion speed is preferably 15μL / min. The coagulation bath is a mixed solution of ethanol and water, and the proportion of ethanol is preferably 50%. A high-performance rare earth photothermal biofiber is obtained. The collected fibers are post-stretched to obtain rare earth photothermal biofibers with good mechanical properties, wherein the post-stretching degree is preferably 600% of the original fiber length.
[0084] Example 4 Preparation of 1.5% NaNdF4@TB rare earth photothermal biofiber by direct doping
[0085] Prepare a formic acid solution of silk fibroin and NaNdF4@TB. The concentration of silk fibroin is preferably 15wt%, the concentration of NaNdF4@TB is preferably 1.5wt%, and CaCl2 and LaCl3 are dissolved in the spinning solution, and their concentrations are preferably 2wt%. The protein solution is extruded into a coagulation bath for wet spinning, and the fibers are collected. The extrusion speed is preferably 15μL / min. The coagulation bath is a mixed solution of ethanol and water, and the proportion of ethanol is preferably 50%. A high-performance rare earth photothermal biofiber is obtained. The collected fibers are post-stretched to obtain rare earth photothermal biofibers with good mechanical properties, wherein the post-stretching degree is preferably 600% of the original fiber length.
[0086] Example 5 Preparation of rare earth photothermal biofibers by in-situ modification during spinning
[0087] Prepare a formic acid solution of silk fibroin. The concentration of silk fibroin is preferably 15wt%, NdCl3 and FeCl2 are dissolved in the spinning solution, the mass fraction of NdCl3 is preferably 2%, and the concentration of FeCl2 is preferably 1%. Add K3Fe(CN)6 to the coagulation bath. Preferably, the mass fraction of K3Fe(CN)6 is 1%. Extrude the protein solution into a coagulation bath for wet spinning, collect fibers, and the extrusion speed is preferably 15 μL / min. The coagulation bath is a mixed solution of ethanol and water, and the proportion of ethanol is preferably 50%. A high-performance rare earth photothermal biofiber is obtained. The collected fibers are post-stretched to obtain rare earth photothermal biofibers with good mechanical properties, wherein the post-stretching degree is preferably 600% of the original fiber length.
[0088] Example 6 Testing of fiber mechanical strength and fiber optical and thermal properties
[0089] The specific test method is as follows: take 8mm of fiber that has been stretched and placed for 24 hours, use Textchno single fiber tensile tester, set the test length to 5mm, clamp the fiber, and stretch it at a speed of 10 mm / min to obtain the tensile value; the fiber diameter is measured by a microscope, the tensile strength is obtained by the ratio of the tensile force to the fiber cross-sectional area, and the tensile curve is obtained by processing with origin software, such as Figure 2~3 As shown ( Figure 2 and Figure 3 In the figure, different curves in the same figure represent the results of multiple repetitions of the same test). It can be seen that the breaking strength of the fibers prepared in Examples 2 and 3 both reached about 500 MPa (Table 1), which can meet the application requirements of equipment heat storage and clothing fabric preparation.
[0090] Take 20 single fibers and twist them into a bundle, and test the photothermal performance under the light of a xenon lamp equipped with a solar spectrum filter. The light intensity used is measured by an optical power meter to be 0.1W / cm 2 The temperature change of the fiber under illumination was tested using a FLIR infrared thermal imaging camera, and the temperature change curve over time was recorded, such as Figures 4 and 5 The results show that the photothermal efficiency of the fibers prepared in Examples 2 to 5 is greater than 40%, which can meet the needs of outdoor active heating and equipment insulation (Table 1).
[0091] Table 1. Test results of fiber mechanical strength and fiber optical and thermal properties
[0092]
[0093] Example 7 Comparison with other fibers
[0094] The breaking strength and breaking elongation of RSF / MoO2NPs hybrid fibers with a content of 0.04 wt% are the best, which are 311.62±10.52 MPa and 153.81±6.21%, respectively (Guo Jianjun. Research on photothermal nanoparticle functionalized silk fibroin composites [D]. Jiangsu University of Science and Technology, 2022. DOI: 10.27171 / d.cnki.ghdcc.2022.000448.).
[0095] RSF-PDA composite fiber, strength 246 MPa, photothermal efficiency 33% (Chen, Wei. , et al. "Polydopamine-Induced Multilevel Engineering of Regenerated Silk Fibroin Fiberfor Photothermal Conversion." Small (Weinheim an der Bergstrasse, Germany)18.11(2022):e2107196).
[0096] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Bioprotein fiber, characterized in that: Includes rare earth nanoparticles and silk fibroin; The rare earth nanoparticles are NaNdF4 modified with Teng's blue or Bruce's blue; The mass ratio of the rare earth photothermal nanoparticles to the silk fibroin is (0.1-1.5): (10-20).
2. The bioprotein fiber according to claim 1, characterized in that: The mass ratio of the rare earth photothermal nanoparticles to the silk fibroin is (0.5-1.5):
15.
3. The bioprotein fiber according to claim 1, wherein the particle size of the rare earth nanoparticles is 180 nm to 220 nm.
4. The method for preparing the biological protein fiber according to claim 1 or 2, characterized in that: The method comprises the following steps: wet spinning the rare earth nanoparticles and silk fibroin in the presence of a cosolvent and an organic acid to obtain the biological protein fiber.
5. The preparation method according to claim 4, characterized in that: The co-solvents include CaCl2 and LaCl3.
6. The preparation method according to claim 4 or 5, characterized in that: The mass ratio of the rare earth nanoparticles, silk fibroin, CaCl2 and LaCl3 is (0.1-1.5):(10-20):2:
2.
7. A photothermal nanocomposite material, characterized in that: It comprises at least one of the biological protein fibers described in any one of claims 1 to 3 and / or the biological protein fibers prepared by the preparation method described in any one of claims 4 to 6 and a matrix thereof.
8. The photothermal nanocomposite material according to claim 7, characterized in that: The substrate includes cloth, resin, rubber, ceramic and / or metal.
9. Application of at least one of the following A) to C) in the field of electrical and / or optical conductors, smart wearables and / or medical bionics: A), the biological protein fiber according to any one of claims 1 to 3; B), biological protein fiber prepared by the preparation method according to any one of claims 4 to 6; C) The photothermal nanocomposite material according to claim 7 or 8.
10. A method for heat preservation and / or heat conduction, characterized in that: Use at least one of the following a) to c) for heat preservation and / or heat conduction: a), the biological protein fiber according to any one of claims 1 to 3; b), biological protein fiber prepared by the preparation method according to any one of claims 4 to 6; c) The photothermal nanocomposite material according to claim 7 or 8.
Citation Information
Patent Citations
Fluorescent salix mongolica regenerated cellulose fibers and preparation method thereof
CN104357931A
Preparation method of regenerated silk protein fiber based on rare-earth / metal ions
CN106435801A
Oriented biological ink based on silk fibroin and preparation method and application thereof
CN112957526A
Near-infrared two-region bifluorescence emission rare earth nano probe as well as preparation method and application thereof
CN115505388A
Sericin nanofiber and method for producing the same, metal ion adsorbent, material with enhanced dyeing function, material with enhanced chemical resistance, and sericin / fibroin composite nanofiber and method for producing the same
JP2012136795A
Cited By
Rare earth ion reinforced silk protein fiber and preparation method thereof
CN119777016A
A rare earth ion-enhanced silk fibroin fiber and its preparation method
CN119777016B