Antibacterial ES fiber for non-woven fabric and preparation process thereof

By adding carbon nanotubes, polyamic acid nanofibers and quaternary ammonium chitosan to PE resin and PET sliced ​​ES fibers, high-efficiency and long-term antibacterial properties are formed, the problem of insufficient antibacterial persistence is solved and the non-existence of the antibacterial life is improved. The antibacterial ability and hygroscopicity of the textile fabric ensure the safety and comfort of medical supplies.

CN119082928APending Publication Date: 2024-12-06福建省福地新材料股份有限公司
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411402595.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The antibacterial effect of existing antibacterial ES fibers is insufficient, resulting in an increased risk of infection in medical adsorbents.

Method used

Use PE resin as the cortical material and PET slice as the core material, and add antibacterial agents to both, including carbon nanotubes, polyamic acid nanofibers and quaternary ammonium chitosan, through the charge of quaternary ammonium chitosan Adsorption and physical sterilization mechanism, the physical puncture effect of carbon nanotubes forms efficient and long-term antibacterial properties, and improves antibacterial durability and hygroscopicity through the high specific surface area and thermal conductivity of polyamic acid nanofibers.

Benefits of technology

It realizes the efficient and long-term antibacterial properties of ES fiber, improves antibacterial durability and hygroscopicity, reduces the probability of wound infection, and accelerates the heat dissipation effect of non-woven fabrics, avoiding the sultry feeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the field of production and processing of textile products, and particularly discloses antibacterial ES fibers for non-woven fabrics and a preparation process of the antibacterial ES fibers. The antibacterial ES fiber for the non-woven fabric comprises a skin layer material and a core layer material in a mass ratio of (1-1.5): 1, and the skin layer material comprises the following raw materials in parts by weight: 10-20 parts of PE resin, 0.2-0.5 part of an antioxidant, 0.1-0.3 part of a dispersing agent, 0.2-0.4 part of an antistatic agent and 2-4 parts of an antibacterial agent; the core layer material comprises the following raw materials in parts by weight: 10-20 parts of PET slices and 2-4 parts of an antibacterial agent; the antibacterial agent comprises the following raw materials in parts by weight: 1-2 parts of carbon nanotubes, 5-10 parts of polyamide acid nanofibers and 3-7 parts of quaternary ammonium salt chitosan. The antibacterial ES fiber has the advantages of being good in antibacterial effect, lasting in antibacterial effect, high in hygroscopicity and fast in heat dissipation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of textile product production and processing, and more specifically, to an antibacterial ES fiber for non-woven fabrics and a preparation process thereof. Background Art

[0002] At present, non-woven fabrics are widely used in the surface layers of sanitary absorbent products and medical surgical products, mainly hot air non-woven fabrics, hot rolled non-woven fabrics and spunbonded non-woven fabrics. When non-woven fabrics are used as the surface layer of absorbent products, they need to be in close contact with the human body, so the non-woven fabrics must be soft, breathable and skin-friendly. The surface layer of disposable absorbent products in the prior art is usually a non-woven fabric made of ES fiber. ES fiber is a composite fiber with a two-component skin-core structure. The skin component has a low melting point and good softness, while the core component has a high melting point and high strength. The non-woven fabric made of ES fiber by hot air or hot rolling is relatively soft and comfortable to use, and because no adhesive is used, it is safer. The first generation of ES fiber was successfully developed by Chisso Corporation of Japan, with its skin layer being PE (polyethylene) and its core layer being PP (polypropylene). PE / PET (polyethylene / polyester) composite ES fiber has now been developed, with its skin layer being PE and its core layer being PET (polyester).

[0003] In the prior art, the Chinese invention patent application document with application number CN2020103231465 discloses an antibacterial and deodorizing ES fiber and a preparation method thereof, wherein the antibacterial and deodorizing ES fiber comprises the following raw material components by weight: 95.5-99.1 parts of HDPE, 100-150 parts of PET, 0-1.5 parts of modified nano ZnO, 0-1.5 parts of modified nano TiO2, and 0-1.5 parts of new activated carbon, wherein the new activated carbon is a polycarboxyl activated carbon obtained by surface oxidation modification and grafting modification. The ES fiber prepared in this way has an antibacterial rate of more than 99.99% against Escherichia coli and Staphylococcus aureus, and has good antibacterial adsorption performance. However, with the passage of time, the antibacterial effect gradually weakens, or even completely fails, and the antibacterial persistence is insufficient. When used in medical adsorption products, such as dressings, it may lead to an increased risk of infection. Summary of the invention

[0004] In order to increase the antibacterial durability of ES fibers for medical absorbent products, the present application provides an antibacterial ES fiber for non-woven fabrics and a preparation process thereof.

[0005] In the first aspect, the present application provides an antibacterial ES fiber for non-woven fabrics, which adopts the following technical solution: An antibacterial ES fiber for non-woven fabrics, comprising a skin layer material and a core layer material in a mass ratio of 1-1.5:1, wherein the skin layer material comprises the following raw materials in parts by weight: 10-20 parts of PE resin, 0.2-0.5 parts of antioxidant, 0.1-0.3 parts of dispersant, 0.2-0.4 parts of antistatic agent and 2-4 parts of antibacterial agent; The core layer material comprises the following raw materials in parts by weight: 10-20 parts of PET chips and 2-4 parts of antibacterial agent; The antibacterial agent comprises the following raw materials in parts by weight: 1-2 parts of carbon nanotubes, 5-10 parts of polyamic acid nanofibers, and 3-7 parts of quaternary ammonium salt chitosan.

[0006] By adopting the above technical scheme, PE resin is used as the skin layer and PET slices are used as the core layer. The skin layer PE has a low melting point and is soft, while the core layer PET has a high melting point and high strength. After the ES fiber is heat-treated, the skin layer can melt and play a bonding role, while the core layer remains in a fiber state, so that it can be formed without an adhesive, which is safer to use. Antibacterial agents are added to both the skin layer and the core layer to increase the antibacterial ability of the ES fiber for non-woven fabrics. Quaternary ammonium chitosan kills microorganisms by destroying the cell walls of microorganisms. The electrostatic interaction between the protonated amino group and the phosphorylated group hinders the nutrient intake and proliferation of the microorganisms. In addition, the positively charged structure of the quaternary ammonium chitosan adsorbs the negatively charged bacterial cell membrane and combines with the negatively charged bacterial cell membrane. , destroying the membrane barrier function, and exerting a bactericidal effect through the conversion of NH / N-Cl, thus showing efficient and long-lasting antibacterial properties. Carbon nanotubes have physical bactericidal effects, can enter bacterial cells, and destroy bacterial cell walls through puncture. Moreover, their hollow tubular structure can also destroy bacterial cells mechanically, thereby improving the antibacterial activity. Moreover, polyamide fibers have a large specific surface area and can load quaternary ammonium chitosan and carbon nanotubes, thereby improving the antibacterial persistence and long-term effect. Moreover, polyamide acid nanofibers and carbon nanotubes have certain hygroscopicity, which can make non-woven fabrics have good tissue fluid adsorption capacity and reduce the probability of wound infection. In addition, carbon nanotubes have good thermal conductivity, which can accelerate the heat dissipation effect of non-woven fabrics, reduce stuffiness, and improve the cool feeling.

[0007] Optionally, the method for preparing the antibacterial agent comprises the following steps: (1) mixing carbon nanotubes and polyamic acid nanofibers uniformly to obtain mixed fibers, adding the mixed fibers to deionized water, adding silica sol and agarose, ultrasonically homogenizing, freeze drying, heating to 300-350° C., and heat treating for 8-10 hours to obtain a porous framework, wherein the mass ratio of the mixed fibers, deionized water, silica sol, and agarose is 1:10-12:3-4:0.16-0.2; (2) impregnating the porous framework with a Tris-HCl buffer solution and a dopamine hydrochloride solution in sequence, washing with deionized water, and drying to obtain a modified porous framework; (3) Add quaternary ammonium salt chitosan to Tris-HCl buffer, add the modified porous framework, immerse at room temperature for 18-20 hours, wash with PBS and distilled water in turn, and dry.

[0008] By adopting the above technical scheme, carbon nanotubes and polyamic acid nanofibers are mixed to obtain a fiber skeleton, which is then dispersed in deionized water. Silica sol and agarose have an adhesion effect, which can increase the adhesion between the fiber and the carbon nanotube overlap in the porous skeleton. After freeze-drying, water molecules sublimate to form pores. During heat treatment, agarose in the porous skeleton is decomposed into water and carbon dioxide by high temperature, and the polyamic acid nanofibers are thermally imidized by heat treatment to form polyimide fibers. The polyimide fibers inside the fiber skeleton are overlapped into a bird's nest structure, and the silica sol can also flow to the fiber overlap during heat treatment to play a secondary bonding role. After the silica sol solidifies, it adheres to the fibers to form a porous skeleton. The surface of the polyimide fiber is hydrophilic, which makes it have a certain hygroscopicity and can absorb and retain a certain amount of water. The carbon nanotube has good liquid absorption capacity because it has a unique nanostructure and surface properties. Due to its high The specific surface area and porous structure can adsorb and store a large amount of liquid, so it has good tissue fluid adsorption capacity, and adsorbs harmful microorganisms on its surface to effectively prevent further infection of the wound; polydopamine is synthesized using dopamine and Tris-HCl buffer, and the catechol it contains provides an effective modification site, showing a strong ability to capture bacteria, and destroys the cell membrane structure of bacteria through ion / protein chelation and electrostatic action. It has unique antibacterial ability and good biocompatibility. It is a very potential antibacterial material and has good adhesion. The self-polymerized polydopamine is evenly distributed on the porous skeleton, with polydopamine as a bridge, combined with quaternary ammonium chitosan. In addition, the porous skeleton structure formed can also facilitate the grafting and loading of quaternary ammonium chitosan, so that the antibacterial agent has a combination of multiple bactericidal mechanisms such as physical sterilization, charge adsorption sterilization of quaternary ammonium chitosan, and bacterial capture of polydopamine, thereby effectively improving the antibacterial performance.

[0009] Optionally, in step (3), heparin is further added to the Tris-HCl buffer, and the mass ratio of heparin to quaternary ammonium salt chitosan is 0.4-0.5:1.

[0010] By adopting the above technical scheme, heparin can be used as a growth factor and anti-inflammatory agent to improve the blood compatibility and biocompatibility of the material. Heparin has high biological activity and can bind to and isolate a variety of growth factors, cytokines and chemokines in the wound site, which can effectively improve wound healing and vascularization, participate in the wound healing process, and reduce inflammation. In addition, heparin's strong electronegativity and microbial interaction effectively improve the antibacterial ability of the antibacterial agent, thereby further improving the antibacterial rate of the antibacterial agent, improving blood compatibility and anti-inflammatory effects, and promoting wound healing.

[0011] Optionally, the preparation method of the polyamic acid nanofiber is: The polyamic acid solution and the boron nitride nanosheets are mixed, and electrospinning is performed after ultrasonic homogenization to obtain a fiber membrane, wherein the mass ratio of the polyamic acid solution to the boron nitride nanosheets is 1:0.2-0.25; The TPU is dissolved to prepare a TPU solution with a concentration of 13-15wt%, and nano-activated carbon and silver nanowires are added to the TPU solution, and ultrasonic homogenization is performed to prepare a blended liquid, wherein the mass ratio of TPU, nano-activated carbon and silver nanowires is 1:0.15-0.2:0.3-0.5; the fiber membrane is placed in the blended liquid, ultrasonically treated for 1-2h, vacuum dried at 60-80°C, cut and crushed to obtain polyamic acid nanofibers with a length of 3-6mm.

[0012] By adopting the above technical scheme, boron nitride nanosheets have excellent thermal conductivity, outstanding mechanical properties, chemical inertness and good antioxidant properties, and they have a high specific surface area, which enables them to interact with bacterial cell membranes, destroy the bacterial cell membranes, and form bacterial silk nets, thereby having certain antibacterial properties. The polyamic acid solution is mixed with the boron nitride nanosheets, and electrospun to form a fiber membrane. The boron nitride nanosheets are evenly arranged in the fiber membrane, thereby improving the antibacterial ability of the fiber membrane, and having good thermal conductivity and heat dissipation effects; silver nanowires are a kind of one-dimensional linear structure with good thermal conductivity and broad-spectrum antibacterial ability, nano-activated carbon has good adsorption, can adsorb bacteria and tissue fluid, TPU is thermoplastic polyurethane, has good flexibility, and is used as a binder, Then, with the assistance of ultrasound, the blended liquid made of TPU, nano-activated carbon and silver nanowires is deposited on the fiber membrane to construct a dense thermal conductive network, ensuring the rapid transfer of heat, and obtaining polyamic acid nanofibers with not only excellent thermal conductivity but also good flexibility and stretchability. The polyamic acid nanofibers can accelerate the dissipation of heat, are not prone to stuffiness, and are relatively cool when used. In addition, due to the addition of boron nitride nanosheets, silver nanowires and nano-activated carbon, the polyamic acid nanofibers have strong antibacterial ability. Moreover, under the adhesion and wrapping effect of TPU, the nano-activated carbon, boron nitride nanosheets and silver nanowires are highly stable on the polyamic acid nanofibers and are not easy to detach, which makes the antibacterial effect lasting. In addition, the nano-activated carbon has a strong adsorption capacity, which can improve the tissue fluid adsorption capacity of the non-woven fabric and improve the moisture absorption effect.

[0013] Optionally, the nano activated carbon and the silver nanowires are both modified with a silane coupling agent.

[0014] By adopting the above technical solution, nano-activated carbon and silver nanowires can be dispersed more evenly in the TPU solution after being treated with a silane coupling agent, thereby adhering evenly to the fiber membrane, thereby improving the thermal conductivity and antibacterial effects of the fiber membrane.

[0015] Optionally, the intrinsic viscosity of the PET chips is 0.7-1dL / g, the PE resin is HDPE, and the melt index is 19-20g / 10min.

[0016] By adopting the above technical solution, PET chips with a specific viscosity and HDPE with a specific melting index are composite spun, so that the prepared ES fiber has better fluffiness, softness and resilience.

[0017] Optionally, the dispersant is selected from at least one of polyethylene glycol, sodium polyacrylate, sodium dodecyl sulfate and fatty alcohol polyoxyethylene ether.

[0018] By adopting the above technical solution, the dispersant can improve the dispersibility and stability of raw materials such as antibacterial agents in the cortical material and improve the processing performance.

[0019] Optionally, the antioxidant is selected from at least one of antioxidant 1010 and antioxidant 168.

[0020] By adopting the above technical solution, the anti-oxidation ability of nanofibers can be improved and their service life can be extended.

[0021] Optionally, the antistatic agent is selected from at least one of ethoxy lauramide, phenol ether phosphate, polyoxyethylene castor oil and polyoxyethylene laurate.

[0022] By adopting the above technical solution, the nanofibers can be prevented from generating static electricity and the adsorption of dust can be reduced.

[0023] In the second aspect, the present application provides a preparation process of antibacterial ES fiber for non-woven fabrics, which adopts the following technical solution: A preparation process of antibacterial ES fiber for non-woven fabrics comprises the following steps: The PE resin is mixed evenly with an antioxidant, a dispersant, an antistatic agent and an antibacterial agent, and melted to obtain a melt to obtain a skin material, and the melting temperature is 210-260°C; The PET slices are dried and mixed evenly with the antibacterial agent, and melted to obtain a melt to obtain a core layer material, and the melting temperature is 270-295°C; According to the mass ratio, the skin layer material and the core layer material are subjected to composite spinning, winding, bundling, stretching, heat setting, curling and cutting to obtain ES fiber. The spinning temperature is 285-290° C. and the cutting length is 38-40 mm.

[0024] By adopting the above technical solution, the skin layer material and the core layer material are mixed and spun to form ES fibers with excellent antibacterial properties, long-lasting antibacterial ability, and certain thermal conductivity and heat dissipation effects.

[0025] In summary, this application has the following beneficial effects: 1. Since the present application adopts PET as the core layer material and PE as the skin layer material, and antibacterial agents are added to both the skin layer and the core layer, the antibacterial agent is made of carbon nanotubes, polyamic acid nanofibers and quaternary ammonium chitosan, which combines the characteristics of carbon nanotubes in adsorbing bacteria, quaternary ammonium chitosan in destroying microbial cell walls to kill microorganisms, and the high specific surface area of ​​polyamic acid nanofibers to form an antibacterial agent with strong antibacterial ability and good long-term antibacterial effect, and obtain ES fiber with excellent antibacterial performance and long-lasting antibacterial effect.

[0026] 2. In the present application, it is preferred to use carbon nanotubes and polyamic acid nanofibers to make mixed fibers, use silica sol and agarose to bond the overlaps, and then heat treat to increase the porosity and produce thermal imidization to obtain a porous skeleton formed by carbon nanotubes and polyimide fibers, and then synthesize polydopamine on its surface, and then use polydopamine as a bridge to load quaternary ammonium salt chitosan, thereby obtaining an antibacterial agent with strong and lasting antibacterial ability.

[0027] 3. In the present application, polyamic acid solution and boron nitride nanosheets are preferably used to form a fiber membrane by electrospinning. The fiber membrane is ultrasonically assisted to be impregnated with a TPU solution containing nano-activated carbon and silver nanowires. The adhesion of TPU is utilized to form a dense heat-conducting and moisture-absorbing network on the fiber membrane, thereby obtaining a polyamic acid fiber with good heat dissipation effect and improved antibacterial ability. DETAILED DESCRIPTION

[0028] The following examples further illustrate the present application in detail.

[0029] Preparation Example 1-15 of Antibacterial Agent In the following preparation examples, the carbon nanotubes have a diameter of 1-2 nm and a length of 10-30 μm, and are selected from Xianfeng Nano, numbered XFS16-1, and item number 105073. The silica sol is selected from Jinan Haiwei Chemical, model HW-02, and the quaternary ammonium salt chitosan is selected from Xi'an Wanfang Biotechnology, item number WFSW-03. Heparin is selected from Anhui Cool Bioengineering, item number GL971501. The preparation method of the polyamic acid solution is as follows: 5 mmol of 4,4'-diaminodiphenyl ether and 80 mL of DMF solution are mixed, stirred for 20 min, 5.05 mmol of pyromellitic anhydride is added, and stirred for 8 h to obtain a polyamic acid solution.

[0030] Preparation Example 1: (1) 20 g of carbon nanotubes and 100 g of polyamic acid nanofibers were mixed uniformly to prepare mixed fibers, the mixed fibers were added to 1440 g of deionized water, 480 g of silica sol and 24 g of agarose, and after ultrasonic homogenization, freeze-dried at -60 ° C for 14 h, heated to 350 ° C, and heat treated for 8 h to obtain a porous skeleton, the mass ratio of the mixed fibers, deionized water, silica sol and agarose was 1:12:4:0.2, and the polyamic acid nanofibers were prepared by electrospinning a polyamic acid solution at a spinning speed of 0.0002 mm / s, a receiving distance of 20 cm, and a voltage of 20 kV; (2) The porous framework was immersed in Tris-HCl buffer (10 mM, pH = 8.5) at room temperature for 10 h, and then immersed in dopamine hydrochloride solution (1 mg / ml) at room temperature for 10 h, washed with deionized water three times, and dried at 60 ° C to obtain a modified porous framework; (3) 70 g of quaternary ammonium salt chitosan and 35 g of heparin were added to 3500 g of Tris-HCl buffer, added to the modified porous framework, immersed at room temperature for 20 h, first washed with PBS (pH 7.4) for 3 times, each for 5 min, then washed with distilled water for 3 times, each for 5 min, and dried at 60°C.

[0031] Preparation Example 2: (1) 10 g of carbon nanotubes and 50 g of polyamic acid nanofibers were mixed uniformly to prepare mixed fibers, the mixed fibers were added to 600 g of deionized water, 180 g of silica sol and 9.6 g of agarose were added, and after ultrasonic homogenization, they were freeze-dried at -60 ° C for 14 h, heated to 300 ° C, and heat treated for 10 h to obtain a porous skeleton, the mass ratio of the mixed fibers, deionized water, silica sol and agarose was 1:10:3:0.16, and the polyamic acid nanofibers were prepared by electrospinning a polyamic acid solution, the spinning speed was 0.0002 mm / s, the receiving distance was 20 cm, and the voltage was 20 kV; (2) The porous framework was immersed in Tris-HCl buffer (10 mM, pH = 8.5) at room temperature for 10 h, and then immersed in dopamine hydrochloride solution (1 mg / ml) at room temperature for 10 h, washed with deionized water three times, and dried at 60 ° C to obtain a modified porous framework; (3) 30 g of quaternary ammonium salt chitosan and 12 g of heparin were added to 1500 g of Tris-HCl buffer, added to the modified porous framework, immersed at room temperature for 18 h, first washed with PBS (pH 7.4) for 3 times, each for 5 min, then washed with distilled water for 3 times, each for 5 min, and dried at 60°C.

[0032] Preparation Example 3: The difference from Preparation Example 1 is that an equal amount of polyamic acid nanofibers are used instead of carbon nanotubes.

[0033] Preparation Example 4: The difference from Preparation Example 1 is that an equal amount of carbon nanotubes is used to replace the polyamic acid nanofibers.

[0034] Preparation Example 5: (1) 20 g of carbon nanotubes and 100 g of polyamic acid nanofibers were mixed uniformly to prepare mixed fibers, and the mixed fibers were added to 1440 g of deionized water, 480 g of silica sol and 24 g of agarose, and after ultrasonic homogenization, freeze-dried, heated to 350° C., and heat treated for 8 h to prepare a porous skeleton, wherein the mass ratio of the mixed fibers, deionized water, silica sol and agarose was 1:12:4:0.2; (2) 70 g of quaternary ammonium salt chitosan and 35 g of heparin were added to 3500 g of Tris-HCl buffer, added to the porous framework, immersed at room temperature for 20 h, first washed with PBS (pH 7.4) for 3 times, each time for 5 min, then washed with distilled water for 3 times, each time for 5 min, and dried at 60°C.

[0035] Preparation Example 6: (1) 20 g of carbon nanotubes and 100 g of polyamic acid nanofibers were mixed uniformly to prepare mixed fibers; (2) the mixed fibers were immersed in a Tris-HCl buffer (10 mM, pH = 8.5) at room temperature for 10 h, and then immersed in a dopamine hydrochloride solution (1 mg / ml) at room temperature for 10 h, washed with deionized water for 3 times, and dried at 60° C. to prepare modified mixed fibers; (3) 70 g of quaternary ammonium salt chitosan and 35 g of heparin were added to 3500 g of Tris-HCl buffer, and the modified mixed fiber was added and immersed at room temperature for 20 h. The fiber was first washed with PBS (pH 7.4) for 3 times, each time for 5 min, and then washed with distilled water for 3 times, each time for 5 min, and dried at 60°C.

[0036] Preparation Example 7: Mix 20g of carbon nanotubes and 100g of polyamic acid nanofibers evenly to prepare mixed fibers, add 70g of quaternary ammonium chitosan and 35g of heparin to 3500g of Tris-HCl buffer, add the mixed fibers, soak at room temperature for 20h, first wash with PBS (pH 7.4) 3 times, 5min each time, then wash with distilled water 3 times, 5min each time, and dry at 60°C.

[0037] Preparation Example 8: The difference from Preparation Example 1 is that heparin is not added in step (3).

[0038] Preparation Example 9: The difference from Preparation Example 1 is that the preparation method of polyamic acid nanofibers is as follows: a polyamic acid solution is mixed with boron nitride nanosheets, and electrospinning is performed after ultrasonic homogenization to obtain a fiber membrane. The boron nitride nanosheets are selected from Suzhou Napu Material Technology, model NS-BN, the mass ratio of polyamide solution to boron nitride nanosheets is 1:0.25, the spinning speed is 0.0002 mm / s, the receiving distance is 20 cm, and the voltage is 20 kV; 13 g of TPU was dissolved in a solvent (DMF and THF in a mass ratio of 1:1) to prepare a TPU solution with a concentration of 15 wt%, nano-activated carbon and silver nanowires were added to the TPU solution, and ultrasonicated at a frequency of 20 kHz for 30 min to prepare a blended liquid, wherein the mass ratio of TPU, nano-activated carbon and silver nanowires was 1:0.2:0.5, TPU was selected from Yantai Wanhua, model WHT-1190, the silver nanowire had a diameter of 70 nm and a length of 45 μm, the nano-activated carbon had a particle size of 20 nm, and both the nano-activated carbon and the silver nanowires were impregnated with a 3 wt% aqueous solution of a silane coupling agent KH550; The fiber membrane was placed in the blended liquid, subjected to ultrasonic treatment at a frequency of 30 kHz for 1 hour, vacuum dried at 60° C., cut and crushed to obtain polyamic acid nanofibers with a length of 6 mm.

[0039] Preparation Example 10: The difference from Preparation Example 1 is that the preparation method of polyamic acid nanofibers is as follows: a polyamic acid solution is mixed with boron nitride nanosheets, and electrospinning is performed after ultrasonic homogenization to obtain a fiber membrane. The boron nitride nanosheets are selected from Suzhou Napu Material Technology, model NS-BN, the mass ratio of polyamide solution to boron nitride nanosheets is 1:0.2, the spinning speed is 0.0002 mm / s, the receiving distance is 20 cm, and the voltage is 20 kV; 13 g of TPU was dissolved in a solvent (DMF and THF in a mass ratio of 1:1) to prepare a TPU solution with a concentration of 13 wt%, nano-activated carbon and silver nanowires were added to the TPU solution, and ultrasonicated at a frequency of 20 kHz for 30 min to prepare a blended liquid, wherein the mass ratio of TPU, nano-activated carbon and silver nanowires was 1:0.15:0.3, TPU was selected from Yantai Wanhua, model WHT-1190, the silver nanowire had a diameter of 70 nm and a length of 45 μm, the nano-activated carbon had a particle size of 20 nm, and both the nano-activated carbon and the silver nanowires were impregnated with a 3 wt% aqueous solution of a silane coupling agent KH550; The fiber membrane was placed in the blended liquid, subjected to ultrasonic treatment at a frequency of 20 kHz for 2 h, vacuum dried at 80° C., cut and crushed to obtain polyamic acid nanofibers with a length of 3 mm.

[0040] Preparation Example 11: The difference from Preparation Example 9 is that the preparation method of polyamic acid nanofibers is as follows: the polyamic acid solution is mixed with boron nitride nanosheets, and the fiber membrane is obtained by electrospinning after ultrasonic homogenization. The boron nitride nanosheets are selected from Suzhou Napu Material Technology, model NS-BN, the mass ratio of polyamide solution to boron nitride nanosheets is 1:0.25, the spinning speed is 0.0002 mm / s, the receiving distance is 20 cm, and the voltage is 20 kV.

[0041] Preparation Example 12: The difference from Preparation Example 9 is that no boron nitride nanosheets are added to the polyamic acid solution during electrospinning.

[0042] Preparation Example 13: The difference from Preparation Example 9 is that no silver nanowires are added.

[0043] Preparation Example 14: The difference from Preparation Example 9 is that no nano-activated carbon is added.

[0044] Preparation Example 15: The difference from Preparation Example 9 is that an equal amount of deionized water is used to replace the TPU solution. Example

[0045] Example 1: An antibacterial ES fiber for non-woven fabrics, comprising a skin layer material and a core layer material with a mass ratio of 1.5:1, the skin layer material comprising 20 kg PE resin, 0.5 kg antioxidant, 0.3 kg dispersant, 0.4 kg antistatic agent and 4 kg antibacterial agent, the PE resin is HDPE, the melt index is 20 g / 10 min, and the density is 0.96 g / cm 3 , selected from Fushun Petrochemical, brand 2911, antioxidant is antioxidant 1010, dispersant is sodium polyacrylate, antistatic agent is ethoxy lauramide, antibacterial agent is made by Preparation Example 1, core layer material includes 20kg PET slices and 4kg antibacterial agent, the intrinsic viscosity of PET slices is 0.7-1dL / g, selected from Qinghua Plastic Factory, Jizhou District, Hengshui City, product number is PET-QH, brand is Qh-pet, antibacterial agent is made by Preparation Example 1.

[0046] The preparation process of the antibacterial ES fiber for non-woven fabrics comprises the following steps: S1. Evenly mix PE resin with antioxidant, dispersant, antistatic agent and antibacterial agent, melt them through a screw extruder to obtain a melt, and prepare a skin material. The temperature of each zone of the screw extruder is: 210°C in zone 1, 220°C in zone 2, 230°C in zone 3, 240°C in zone 4, 250°C in zone 5, and 260°C in zone 6; S2, after drying the PET slices, mix them evenly with the antibacterial agent, melt them through a screw extruder to obtain a melt, and make a core layer material. The temperatures of each zone of the screw extruder are: 270°C in zone 1, 275°C in zone 2, 288°C in zone 3, 295°C in zone 4, 295°C in zone 5, and 295°C in zone 6; S3. According to the mass ratio of skin material: core material of 1.5:1, the skin material and the core material are subjected to composite spinning, winding, bundling, stretching, heat setting, curling and cutting to obtain ES fiber. The spinning temperature is 285°C, the cutting length is 38mm, the side blowing temperature is 14°C, the side blowing humidity is 80%, the main pressure of the curling machine is 0.12MPa, the side pressure is 0.14MPa, the back pressure is 0.08MPa, the winding speed is 1.1kg / min, the stretching multiple is 3.8, the stretching temperature is 75°C, and the heat setting temperature is 110°C for zone 1, 105°C for zone 2, and 105°C for zone 3.

[0047] Example 2: An antibacterial ES fiber for non-woven fabrics, comprising a skin layer material and a core layer material in a mass ratio of 1:1, the skin layer material comprising 10 kg PE resin, 0.2 kg antioxidant, 0.1 kg dispersant, 0.2 kg antistatic agent and 2 kg antibacterial agent, the PE resin is HDPE, the melt index is 20 g / 10 min, and the density is 0.96 g / cm 3 , selected from Fushun Petrochemical, brand 2911, antioxidant is antioxidant 1010, dispersant is sodium polyacrylate, antistatic agent is ethoxy lauramide, antibacterial agent is made by Preparation Example 2, core layer material includes 10kg PET slices and 2kg antibacterial agent, the intrinsic viscosity of PET slices is 0.7-1dL / g, selected from Qinghua Plastic Factory, Jizhou District, Hengshui City, product number is PET-QH, brand is Qh-pet, antibacterial agent is made by Preparation Example 2.

[0048] The preparation process of the antibacterial ES fiber for non-woven fabrics comprises the following steps: S1. Evenly mix PE resin with antioxidant, dispersant, antistatic agent and antibacterial agent, melt them through a screw extruder to obtain a melt, and prepare a skin material. The temperature of each zone of the screw extruder is: 210°C in zone 1, 220°C in zone 2, 230°C in zone 3, 240°C in zone 4, 250°C in zone 5, and 260°C in zone 6; S2, after drying the PET slices, mix them evenly with the antibacterial agent, melt them through a screw extruder to obtain a melt, and make a core layer material. The temperatures of each zone of the screw extruder are: 270°C in zone 1, 275°C in zone 2, 288°C in zone 3, 295°C in zone 4, 295°C in zone 5, and 295°C in zone 6; S3. According to the mass ratio of skin material: core material of 1:1, the skin material and the core material are subjected to composite spinning, winding, bundling, stretching, heat setting, curling and cutting to obtain ES fiber. The spinning temperature is 290°C, the cutting length is 40mm, the side blowing temperature is 14°C, the side blowing humidity is 80%, the main pressure of the curling machine is 0.12MPa, the side pressure is 0.14MPa, the back pressure is 0.08MPa, the winding speed is 1.1kg / min, the stretching multiple is 3.8, the stretching temperature is 75°C, and the heat setting temperature is 110°C for zone 1, 105°C for zone 2, and 105°C for zone 3.

[0049] Example 3: An antibacterial ES fiber for non-woven fabrics, comprising a skin layer material and a core layer material in a mass ratio of 1:1, the skin layer material comprising 15 kg PE resin, 0.4 kg antioxidant, 0.2 kg dispersant, 0.3 kg antistatic agent and 3 kg antibacterial agent, the PE resin is HDPE, the melt index is 20 g / 10 min, and the density is 0.96 g / cm 3 , selected from Fushun Petrochemical, brand 2911, antioxidant is antioxidant 1010, dispersant is sodium polyacrylate, antistatic agent is ethoxy lauramide, antibacterial agent is made by Preparation Example 1, core layer material includes 15kg PET slices and 3kg antibacterial agent, the intrinsic viscosity of PET slices is 0.7-1dL / g, selected from Hengshui Jizhou District Qinghua Plastic Factory, product number is PET-QH, brand is Qh-pet, antibacterial agent is made by Preparation Example 2.

[0050] The preparation process of the antibacterial ES fiber for non-woven fabrics comprises the following steps: S1. Evenly mix PE resin with antioxidant, dispersant, antistatic agent and antibacterial agent, melt them through a screw extruder to obtain a melt, and prepare a skin material. The temperature of each zone of the screw extruder is: 210°C in zone 1, 220°C in zone 2, 230°C in zone 3, 240°C in zone 4, 250°C in zone 5, and 260°C in zone 6; S2, after drying the PET slices, mix them evenly with the antibacterial agent, melt them through a screw extruder to obtain a melt, and make a core layer material. The temperatures of each zone of the screw extruder are: 270°C in zone 1, 275°C in zone 2, 288°C in zone 3, 295°C in zone 4, 295°C in zone 5, and 295°C in zone 6; S3. According to the mass ratio of skin material: core material of 1:1, the skin material and the core material are subjected to composite spinning, winding, bundling, stretching, heat setting, curling and cutting to obtain ES fiber. The spinning temperature is 290°C, the cutting length is 38mm, the side blowing temperature is 14°C, the side blowing humidity is 80%, the main pressure of the curling machine is 0.12MPa, the side pressure is 0.14MPa, the back pressure is 0.08MPa, the winding speed is 1.1kg / min, the stretching multiple is 3.8, the stretching temperature is 75°C, and the heat setting temperature is 110°C for zone 1, 105°C for zone 2, and 105°C for zone 3.

[0051] Preparation Example 4: An antibacterial ES fiber for non-woven fabric, which differs from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 5.

[0052] Example 5: An antibacterial ES fiber for non-woven fabric, which differs from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 6.

[0053] Example 6: An antibacterial ES fiber for non-woven fabric, which differs from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 7.

[0054] Example 7: An antibacterial ES fiber for non-woven fabrics, which differs from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 8.

[0055] Example 8: An antibacterial ES fiber for non-woven fabrics, which differs from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 9.

[0056] Example 9: An antibacterial ES fiber for non-woven fabric, which differs from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 10.

[0057] Example 10: An antibacterial ES fiber for non-woven fabrics, which differs from Example 8 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 11.

[0058] Example 11: An antibacterial ES fiber for non-woven fabrics, which differs from Example 8 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 12.

[0059] Example 12: An antibacterial ES fiber for non-woven fabric, which differs from Example 8 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 13.

[0060] Example 13: An antibacterial ES fiber for non-woven fabric, which differs from Example 8 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 14.

[0061] Example 14: An antibacterial ES fiber for non-woven fabric, which differs from Example 8 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 15.

[0062] Comparative Example Comparative Example 1: An antibacterial ES fiber for non-woven fabric, which is different from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 3.

[0063] Comparative Example 2: An antibacterial ES fiber for non-woven fabric, which is different from Example 1 in that the antibacterial agent in the skin layer material and the core layer material is made from Preparation Example 4.

[0064] Comparative Example 3: An antibacterial ES fiber for non-woven fabric, which differs from Example 1 in that quaternary ammonium salt chitosan is used as an antibacterial agent.

[0065] Comparative Example 4: Commercially available ES fiber nonwoven fabric, item number KHJK-1, selected from Zhejiang Hengyue New Materials.

[0066] Performance testing ES fibers were prepared according to the methods in the examples and comparative examples, and performance tests were performed according to the following methods. The test results are recorded in Table 1.

[0067] 1. Antibacterial rate: The test was carried out in accordance with GB15979-2002 "Hygiene Standards for Disposable Hygiene Products", and the test bacteria were Staphylococcus aureus (ATCC6538), Candida albicans (ATCC10231) and Escherichia coli (8099). The antibacterial rate was then tested again after storage at room temperature (25°C and 65% relative humidity) for 6 months. 2. Breaking strength: Tested in accordance with GB / T14337-2008 "Test method for tensile properties of chemical staple fibers".

[0068] 3. Wicking height: Use LFY-215 fabric capillary effect tester to test the wicking height of the fiber. Fix the fiber on the instrument, add water to the sink, and test for 30 minutes.

[0069] 4. Thermal conductivity: Use DRL-III thermal conductivity meter to test the thermal conductivity of the fiber.

[0070] Table 1 Performance test of antibacterial ES fiber for nonwoven fabrics Combined with the data in Table 1 and Examples 1-3, the antibacterial agent prepared in Preparation Example 1 and Preparation Example 2 is used in the core layer material and the skin layer material to effectively increase the antibacterial ability of the ES fiber, and has a strong long-term antibacterial property. After being stored at room temperature for 6 months, it still has a strong antibacterial property, and has high breaking strength, good mechanical properties, large wicking height, good liquid absorption effect, good heat transfer, and is not easy to produce stuffiness.

[0071] Comparative Examples 1 and 2 respectively use the antibacterial agents prepared in Preparation Examples 3 and 4. Compared with Preparation Example 1, Preparation Examples 3 and 4 only use polyamic acid fibers and carbon nanotubes, respectively. The data in Table 1 show that the ES fiber prepared in Comparative Example 1 has a significantly lower infection coefficient, a reduced cool feeling, a weakened antibacterial ability, and poor antibacterial durability. Although the breaking strength is improved, the wicking height is reduced and the hygroscopicity is weakened. Although the antibacterial ability and thermal conductivity of the ES fiber prepared in Comparative Example 2 are improved, the durability is weakened and the breaking strength is reduced.

[0072] In Comparative Example 3, only quaternary ammonium salt chitosan was used as the antibacterial agent. The data in Table 1 showed that the antibacterial ability decreased, the durability became worse, and the mechanical strength and heat dissipation effect were reduced.

[0073] Comparative Example 5 is a commercially available non-woven fabric, which has no antibacterial ability, general mechanical properties, no heat dissipation effect, and poor cooling feeling.

[0074] In Example 4, the antibacterial agent prepared in Preparation Example 5 was used. Compared with Preparation Example 1, polydopamine was not formed on the porous skeleton. It can be seen that the antibacterial ability of the ES fiber was reduced, and the antibacterial persistence was weakened. The wicking height was slightly reduced, indicating that polydopamine can increase the antibacterial persistence of quaternary ammonium salt chitosan and improve the adsorption capacity of ES fiber to tissue fluid.

[0075] In Example 5, the antibacterial agent prepared in Preparation Example 6 was used. Compared with Example 1, silica sol and agarose were not used to construct the porous skeleton. It can be seen that the antibacterial persistence of ES fibers was reduced, indicating that mixing polyamic acid nanofibers and carbon nanotubes to prepare a porous skeleton can prolong the release time of quaternary ammonium salt chitosan.

[0076] In Example 6, the antibacterial agent prepared by Preparation Example 7 was prepared by only mixing the raw materials evenly and then immersing them at room temperature. It can be seen that its antibacterial performance decreased, the antibacterial durability weakened, and the hygroscopicity decreased.

[0077] Compared with Example 1, Example 7 uses the ES fiber prepared in Preparation Example 8 without adding heparin. Table 1 shows that the antibacterial ability of the ES fiber prepared in Example 7 decreases and the wicking height weakens, indicating that heparin can increase the antibacterial ability and mixed hygroscopicity of the ES fiber.

[0078] In Example 8 and Example 9, the antibacterial agents prepared in Preparation Example 9 and Preparation Example 10 were used respectively. Compared with Preparation Example 1, a certain amount of boron nitride nanosheets, silver nanowires and other raw materials were added when preparing polyamic acid nanofibers in Preparation Example 9 and Preparation Example 10. Table 1 shows that the antibacterial ability of the ES fibers prepared in Example 8 and Example 9 is improved, the antibacterial long-term effect is improved, the liquid absorption effect is enhanced, and the mechanical strength is improved.

[0079] In Example 10, the antibacterial agent prepared in Preparation Example 11 was used. Compared with Preparation Example 9, Preparation Example 11 only used boron nitride nanosheets and polyamic acid solution to prepare polyamic acid nanofibers. It can be seen from the data in Table 1 that compared with Examples 8 and 9, the antibacterial rate of ES fibers decreased significantly, and the breaking strength was significantly reduced, the wicking height was reduced, the liquid absorption capacity was reduced, the heat transfer coefficient was reduced, and the heat dissipation effect was worse.

[0080] In Example 11, the antibacterial agent prepared in Preparation Example 12 is used. Compared with Preparation Example 9 in Example 8, no boron nitride nanosheets are added in Preparation Example 12, and the fiber membrane prepared by electrospinning of a polyamic acid solution is placed in the blending liquid and immersed in ultrasound. The heat transfer coefficient of the polyamic acid nanofibers thus prepared decreases, the heat dissipation effect becomes worse, the cooling feeling is weakened, and the antibacterial rate is significantly reduced.

[0081] Compared with Example 8, Example 12 uses the antibacterial agent prepared in Preparation Example 13, in which no silver nanowires are added. As shown in Table 1, the heat dissipation effect is reduced and the antibacterial rate is worsened.

[0082] In Example 13, the antibacterial agent prepared in Preparation Example 14 was used. Compared with Example 8, no nano-activated carbon was added when preparing the blended liquid. It can be seen that the antibacterial rate of the ES fiber decreased and the moisture absorption effect became worse.

[0083] In Example 14, the antibacterial agent prepared in Preparation Example 15 was used. Compared with Example 8, deionized water was used instead of TPU. It can be seen that the antibacterial durability of the ES fiber is deteriorated, and the breaking strength and mechanical properties are reduced.

[0084] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An antibacterial ES fiber for nonwoven fabrics, characterized in that: The invention comprises a skin layer material and a core layer material in a mass ratio of 1-1.5:1, wherein the skin layer material comprises the following raw materials in parts by weight: 10-20 parts of PE resin, 0.2-0.5 parts of antioxidant, 0.1-0.3 parts of dispersant, 0.2-0.4 parts of antistatic agent and 2-4 parts of antibacterial agent; The core layer material comprises the following raw materials in parts by weight: 10-20 parts of PET chips and 2-4 parts of antibacterial agent; The antibacterial agent comprises the following raw materials in parts by weight: 1-2 parts of carbon nanotubes, 5-10 parts of polyamic acid nanofibers, and 3-7 parts of quaternary ammonium salt chitosan.

2. The antibacterial ES fiber for nonwoven fabric according to claim 1, characterized in that: The preparation method of the antibacterial agent comprises the following steps: (1) The carbon nanotubes and polyamic acid nanofibers are mixed uniformly to obtain mixed fibers, the mixed fibers are added to deionized water, silica sol and agarose are added, ultrasonically homogenized, freeze-dried, heated to 300-350°C, and heat treated for 8-10 hours to obtain a porous skeleton, wherein the mass ratio of the mixed fibers, deionized water, silica sol and agarose is 1:10-12:3-4:0.16-0.2; (2) impregnating the porous framework with a Tris-HCl buffer solution and a dopamine hydrochloride solution in sequence, washing with deionized water, and drying to obtain a modified porous framework; (3) Add quaternary ammonium salt chitosan to Tris-HCl buffer, add the modified porous skeleton, immerse at room temperature for 18-20 hours, wash with PBS and distilled water in turn, and dry.

3. The antibacterial ES fiber for nonwoven fabric according to claim 2, characterized in that: In the step (3), heparin is also added to the Tris-HCl buffer, and the mass ratio of heparin to quaternary ammonium salt chitosan is 0.4-0.5:

1.

4. The antibacterial ES fiber for nonwoven fabric according to claim 1, characterized in that: The preparation method of the polyamic acid nanofiber: The polyamic acid solution and the boron nitride nanosheets are mixed, and electrospinning is performed after ultrasonic homogenization to obtain a fiber membrane, wherein the mass ratio of the polyamic acid solution to the boron nitride nanosheets is 1:0.2-0.25; The TPU is dissolved to prepare a TPU solution with a concentration of 13-15wt%, and nano-activated carbon and silver nanowires are added to the TPU solution, and ultrasonically homogenized to prepare a blended solution, wherein the mass ratio of the TPU, the nano-activated carbon and the silver nanowires is 1:0.15-0.2:0.3-0.5; The fiber membrane is placed in the blended liquid, subjected to ultrasonic treatment for 1-2 hours, vacuum dried at 60-80° C., cut and crushed to obtain polyamic acid nanofibers with a length of 3-6 mm.

5. The antibacterial ES fiber for nonwoven fabric according to claim 4, characterized in that: The nano activated carbon and the silver nanowires are both modified by a silane coupling agent.

6. The antibacterial ES fiber for nonwoven fabric according to claim 1, characterized in that: The intrinsic viscosity of the PET chips is 0.7-1dL / g, the PE resin is HDPE, and the melt index is 19-20g / 10min.

7. The antibacterial ES fiber for nonwoven fabric according to claim 1, characterized in that: The dispersant is selected from at least one of polyethylene glycol, sodium polyacrylate, sodium dodecyl sulfonate and fatty alcohol polyoxyethylene ether.

8. The antibacterial ES fiber for nonwoven fabric according to claim 1, characterized in that: The antioxidant is selected from at least one of the antioxidant 1010 and the antioxidant 168 .

9. The antibacterial ES fiber for nonwoven fabric according to claim 1, characterized in that: The antistatic agent is selected from at least one of ethoxy lauramide, phenol ether phosphate, polyoxyethylene castor oil and polyoxyethylene laurate.

10. The process for preparing the antibacterial ES fiber for nonwoven fabric according to any one of claims 1 to 9, characterized in that: The following steps are involved: The PE resin is mixed evenly with an antioxidant, a dispersant, an antistatic agent and an antibacterial agent, and melted to obtain a melt to obtain a skin material, and the melting temperature is 210-260°C; The PET slices are dried and mixed evenly with the antibacterial agent, and melted to obtain a melt to obtain a core layer material, and the melting temperature is 270-295°C; According to the mass ratio, the skin layer material and the core layer material are subjected to composite spinning, winding, bundling, stretching, heat setting, curling and cutting to obtain ES fiber. The spinning temperature is 285-290° C. and the cutting length is 38-40 mm.

Citation Information

Cited By

  • Probiotic hygienic product and preparation method thereof

    CN119345439A

  • Antibacterial flexible sheath-core composite fiber and preparation method thereof