Manufacturing process of industrial washing resistant tooling fabric

Through the warp sizing and shaft weaving, tension-free desizing, door Fuji shaping and water-splashing finishing processes of tooling fabrics, combined with specific fibers and dye combinations, the problem of insufficient color fastness and dimensional stability of tooling fabrics in industrial washing is solved. Achieve significant improvement in the service life and stability of the fabric.

CN119082988APending Publication Date: 2024-12-06HUAMAO (XIAMEN) WEAVING DYEING & FINISHING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411414068.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing tooling fabrics have insufficient color fastness and dimensional stability during industrial washing, especially dye pollution and high-temperature color modification during dyeing process, which leads to spandex instability, affecting the multiple service life of the fabric.

Method used

Using a process of industrial washing-resistant tooling fabric production, including warp sizing and shaft weaving, tension-free desizing, door Fuji shaping and water-splashing, and weaving with pigmented polyester/nylon raw liquid coloring fiber and core-encapsulated elastic yarn combined with Carbon black or inorganic dyes coated with silicon-based fluorine-free waterproofing agents and chitosan compositions are calendered or bonded to improve the elasticity and stability of the fabric.

Benefits of technology

The color fastness and dimensional stability of the fabric are significantly improved, the elongation of the weft elasticity reaches more than 18%, the resilience of the weft elasticity is more than 97%, and the color fastness of the 75-degree 50 washes reaches more than 4 levels, and the dimensional stability is Within ±1.2%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082988A_ABST
    Figure CN119082988A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing process of a tooling fabric resistant to industrial washing, and relates to the technical field of textile fabrics, and the manufacturing process comprises the following steps: step 1, warping and sizing, and re-beaming and weaving; step 2, carrying out tension-free desizing; step 3, carrying out centrally-fixed drying; step 4, water sprinkling and finishing; wherein the warp yarns are pigment type polyester / nylon stock solution colored fibers or core-spun elastic yarns; the weft yarns are pigment type polyester / nylon stock solution colored fibers and / or core-spun elastic yarns; the core-spun elastic yarn is formed by coating polyolefin elastic yarn with pigment type polyester / nylon stock solution colored fiber, and the polyolefin elastic yarn accounts for 8-24 wt% of the weight of the core-spun elastic yarn. The pigment type polyester / nylon stock solution colored fiber contains a coloring agent with the weight percentage of 0.1-8 wt%; the polyolefin elastic yarn is obtained by mixing first matrix resin and second matrix resin according to the mass ratio of 1: (0.5-2) and then carrying out melt spinning. The method has the effect of remarkably improving the color fastness and the dimensional stability of the tooling fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of textile fabrics, and in particular to a process for manufacturing workwear fabrics resistant to industrial washing. Background Art

[0002] As consumers' requirements for wearing comfort continue to increase, "no elasticity, no fabric" has almost become an industry consensus. Wearing comfortable and practical clothing in the workplace is becoming an indispensable need. Workwear is a rapidly developing industry, and workers' needs for it have changed. How to make workwear comfortable and elastic, and reuse it many times without losing its functional properties, and keep its shape after washing, extending its life cycle. Not only can it be worn at work, it is also suitable for various occasions, such as outdoor activities, sports and vacations.

[0003] Currently, Industrial Washing ISO15797 / Industrial Washing EN ISO 20471 is a standard used in the textile industry. It involves the durability and stability requirements of textiles during industrial washing, including indicators such as dimensional stability, color fastness and appearance quality after washing. This standard is suitable for textiles that need to be frequently washed industrially, such as bedding and work clothes in the hotel and medical industries. The number of washings can reach 50-100 times.

[0004] The combination of polyester / nylon and other chemical fiber filaments with spandex is currently a common material combination and choice for increasing fabric elasticity and wearing comfort. However, there are still some shortcomings in terms of color fastness to washing and dimensional stability. Especially during the dyeing process, the dye will contaminate the spandex, causing the spandex to absorb the dye and affect the color fastness of the fabric. At the same time, multiple high-temperature color corrections will cause the spandex to be unstable. During the process washing stage, high-temperature washing is required at a temperature of 75°C, which will cause the spandex to deform and reduce the dimensional stability of the fabric, which needs to be improved. Summary of the invention

[0005] In view of this, the purpose of this application is to provide a process for manufacturing industrial washable workwear fabrics to achieve the purpose of significantly improving color fastness and dimensional stability. The specific scheme is as follows:

[0006] A process for producing industrial washable workwear fabric comprises the following steps:

[0007] Step 1, warping, sizing and weaving: warp yarn is based on yarn specifications, above 70D is free of sizing, below 70D is sizing and waxing; weft yarn is sizing and then weaving; finally, warp yarn and weft yarn are woven;

[0008] Step 2, tension-free desizing: the fabric obtained by weaving treatment is dyed and finished by direct casting, which is used to stimulate the elasticity of the fabric so that it can fully shrink in the latter stage;

[0009] Step 3, mid-setting and drying: using Monforts setting machine;

[0010] Step 4: Splash water to finish: Use splash water agent;

[0011] Wherein, the warp yarn is a pigmented polyester / nylon solution-dyed fiber or a core-spun stretch yarn; the weft yarn is a pigmented polyester / nylon solution-dyed fiber and / or a core-spun stretch yarn; the core-spun stretch yarn is composed of a pigmented polyester / nylon solution-dyed fiber coated with a polyolefin stretch yarn, and the weight percentage of the polyolefin stretch yarn in the core-spun stretch yarn is 8-24wt%; the pigmented polyester / nylon solution-dyed fiber contains a colorant in an amount of 0.1-8wt% by weight; the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2.

[0012] Preferably: it also includes the steps of calendering, coating or laminating the fabric after water splashing finishing; the calendering is carried out through the calendering process, controlling the temperature to 140°C, the speed to 20m / min, the pressure to 120N / mm, and then transferring the moisture-permeable base glue and the surface glue for finishing; the laminating finishing is carried out by laminating with a hot melt adhesive engraving roller, and controlling the temperature to 40-60°C for aging for 24 hours.

[0013] Preferably: the first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling group, an acyl chloride group or a sulfonic acid group; and the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a thiol group or anhydride group.

[0014] Preferably: the colorant is carbon black or inorganic dye coated with a chitosan composition; the chitosan composition accounts for 10-50wt% of the colorant by weight; the particle size of the carbon black or inorganic dye is 2-15μm; the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black or inorganic dye and the chitosan composition.

[0015] Preferably, the chitosan composition is prepared by mixing chitosan, a silane coupling agent, a binary or multi-polymer of ethylene and butene or octene, polyacrylate and / or polyacrylic acid ester, and methyl vinyl silicone oil in a weight ratio of 12-16:2-4:1-5:2-3:0.2-0.8.

[0016] Preferably, the carbon black is obtained by grafting hydroxymethyl carbon black with maleic anhydride.

[0017] Preferably: the warp yarn is the first yarn, the first yarn is polyester stock black DTY 75 / 72SD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is S-direction yarn; the weft yarn is the first yarn and the second yarn, the second yarn is polyester stock black ATY 340 / 144SD, and the density of the weft yarn is 164 strands / inch, the weft density is 144 strands / inch, and the gram weight is 275g / square meter; in step 1, the warping machine arranges the warp yarn evenly and forms a whole shaft 1008 whole shaft, without sizing, and then forms a weaving shaft 1008*9; the loom adopts a double-nozzle machine, and hangs the first yarn on the first creel, and hangs the second yarn on the second creel, controls the rotation speed of the loom to 450rpm, and forms a first organization form with 8*12 coordinates to weave to obtain a first fabric, wherein the weft directions 1, 2, 3, 5, 7, 8, 9, 11 are the corresponding first yarns, and 4, 6, 10, 12 are the second yarns.

[0018] Preferably: the warp yarn is the third yarn, the third yarn is nylon liquid black DTY 70 / 68FD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is Z-direction yarn; the weft yarn is the fourth yarn and the fifth yarn, the fourth yarn is nylon liquid black DTY 70 / 68FD and polyolefin stretch yarn 42D, and the draft ratio of the core is 3.3, the twist is 800, and the twist direction is Z-direction yarn; the fifth yarn is double-strand nylon liquid black DTY 140 / 136FD, and the density of the weft yarn is 158 strands / inch, the weft density is 156 strands / inch, and the gram weight is 250g / square meter; in step 1, the warping machine arranges the warp yarn evenly and forms a whole shaft of 1100 whole shafts, the sizing yarn is waxed, and then combined into a weaving shaft of 1100*8; the loom adopts a double-nozzle machine, and the fourth yarn is hung on the third creel, and the fifth yarn is hung on the fourth creel, the speed of the loom is controlled to be 450rpm, and the second fabric is woven in a second organizational form with 10*15 coordinates, wherein the weft directions 1, 2, 4, 5, 7, 8, 10, 11, 13, 14 are the corresponding fourth yarns, and 3, 6, 9, 12, 15 are the fifth yarns.

[0019] Preferably: the warp yarn is the sixth yarn, the sixth yarn is nylon stock solution gray DTY 140 / 96SD and polyolefin stretch yarn 105D, and the draft ratio of the core is 3.8, the twist is 700, and the twist direction is Z-direction yarn; the weft yarn is the sixth yarn and the seventh yarn, the seventh yarn is nylon stock solution gray ATY 160 / 96FD, and the density of the weft yarn is 106 yarns / inch, the weft density is 144 yarns / inch, and the gram weight is 268g / square meter; in step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1008 whole shaft, without sizing, and then forms a weaving shaft 1008*6; the loom adopts a double-nozzle machine, and hangs the sixth yarn on the fifth creel, and hangs the seventh yarn on the sixth creel, controls the speed of the loom to 450rpm, and forms a third organization form with 6*12 coordinates to weave to obtain a third fabric, wherein the weft directions 1, 3, 5, 7, 9, 11 are the corresponding sixth yarns, and 2, 4, 6, 8, 10, 12 are the seventh yarns.

[0020] Preferably: the temperature of the Monfushi setting machine is controlled at 180°C, the speed is 40m / min, and the overfeed is 3%-22%; and in step 4, a silicon-based fluorine-free waterproof agent is used as a water-repellent agent in the Monfushi setting machine, the temperature is controlled at 180°C, the speed is 30m / min, the overfeed is 3%-22%, and then the oven is used for heat setting for 1-3min, and the drying temperature is controlled to 100°C.

[0021] It can be seen from the above scheme that the present application provides a process for producing industrial water-washing resistant workwear fabrics, which has the effect of significantly improving the color fastness and dimensional stability of the fabrics; based on the weft elastic elongation, it reaches more than 18%, based on FZ / T01062-1999, the weft elastic recovery of the fabric is more than 97%, based on EN ISO 20471:2013+A1:2016Clause 5.3.3, ISO 105-C06:2010, the color fastness of the fabric after 50 washes at 75 degrees is above level 4, and based on EN ISO 20471:2013+A1:2016Clause5.4, the dimensional stability is within ±1.2%. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0023] Figure 1 This is a schematic diagram of the structure of the first organizational form disclosed in this application;

[0024] Figure 2 A schematic diagram of the structure of the second organizational form disclosed in this application;

[0025] Figure 3 This is a schematic diagram of the structure of the third organizational form disclosed in this application. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0027] It should be mentioned that the industrial washable workwear fabric production process of the present application adopts a loom during the weaving process, and the loom controls the up and down movement of the heald frame on the loom through a set small jacquard computer heald program to form a warp opening, which is interwoven with the weft yarn to form a cloth surface with a small jacquard effect.

[0028] Inorganic dye is sulfate, phosphate, silicate, carbonate, sulfide, metal etc., and the inorganic dye adopted in the present application embodiment is based on silicate.Due to the less selection difference of dye, it is not repeated here.Meanwhile, the multipolymer in the present application embodiment is a small molecular weight multipolymer, and general molecular weight is less than 2000, and maximum will not exceed 3000, and the multipolymer of large molecular weight is not suitable for being used, and the difference of small molecule multipolymer is less, it is not repeated here.

[0029] The following is a detailed description of the manufacturing process of the industrial washable workwear fabric of the present application.

[0030] A process for producing industrial washable workwear fabric comprises the following steps:

[0031] Step 1, warping, sizing and weaving: warp yarn is based on yarn specifications, above 70D is free of sizing, below 70D is sizing and waxing; weft yarn is sizing and then weaving; finally, warp yarn and weft yarn are woven;

[0032] Step 2, tension-free desizing: the fabric obtained by weaving treatment is dyed and finished by direct casting, which is used to stimulate the elasticity of the fabric so that it can fully shrink in the latter stage;

[0033] Step 3, mid-setting and drying: using Monforts setting machine;

[0034] Step 4: Splash water to finish: Use splash water agent;

[0035] in:

[0036] The warp yarn is pigmented polyester / nylon solution-dyed fiber or core-spun stretch yarn.

[0037] The weft yarn is a pigmented polyester / nylon solution-dyed fiber and / or a core-spun stretch yarn. Based on this, when the weft yarn is selected from three different forms of pigmented polyester / nylon solution-dyed fiber, core-spun stretch yarn, or a combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn, the color fastness and dimensional stability can be improved, and when the combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn is used, the color fastness and dimensional stability effect is more significant.

[0038] It should be noted that the core-spun stretch yarn is composed of a polyolefin stretch yarn coated with a pigmented polyester / nylon solution-dyed fiber, and the weight percentage of the polyolefin stretch yarn in the core-spun stretch yarn is 8-24wt%. The pigmented polyester / nylon solution-dyed fiber contains a colorant in a weight percentage of 0.1-8wt%, and the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2. The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling group, an acyl chloride group or a sulfonic acid group; and the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a mercapto group or an anhydride group.

[0039] The temperature of the Monfushi setting machine is controlled at 180°C, the speed is 40m / min, and the overfeed is 3%-22%. In step 4, a silicon-based fluorine-free waterproof agent is used as a water-splashing agent in the Monfushi setting machine, and the temperature is controlled at 180°C, the speed is 30m / min, and the overfeed is 3%-22%. Then, the oven is used for heat setting for 1-3 minutes, and the drying temperature is controlled at 100°C.

[0040] In order to further improve the color fastness and dimensional stability of the fabric, thereby increasing the application options and scope of the fabric, the fabric that has been water-splashed can also be calendered, coated or laminated. Among them, calendering is to use a calendering process with a controlled temperature of 140°C, a speed of 20m / min, and a pressure of 120N / mm, and then transfer coating based on a moisture-permeable base adhesive and a surface adhesive; the laminating process is to use a hot melt adhesive engraved roller lamination process, and control the temperature at 40-60°C for aging for 24 hours.

[0041] It should be mentioned that the colorant is carbon black or inorganic dye coated with a chitosan composition. The chitosan composition accounts for 10-50wt% of the colorant by weight. The particle size of the carbon black or inorganic dye is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black or inorganic dye with the chitosan composition. Wherein, the chitosan composition is composed of chitosan, a silane coupling agent, a binary or multi-polymer of ethylene and butene or octene, polyacrylate and / or polyacrylic acid vinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 12-16:2-4:1-5:2-3:0.2-0.8. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0042] Embodiment 1

[0043] A process for producing industrial washable workwear fabric comprises the following steps:

[0044] Step 1, warping, sizing and weaving: warp yarn is based on yarn specifications, above 70D is free of sizing, below 70D is sizing and waxing; weft yarn is sizing and then weaving; finally, warp yarn and weft yarn are woven;

[0045] Step 2, tension-free desizing: the fabric obtained by weaving treatment is dyed and finished by direct casting, which is used to stimulate the elasticity of the fabric so that it can fully shrink in the latter stage;

[0046] Step 3, mid-setting and drying: using Monforts setting machine;

[0047] Step 4: Splash water to finish: Use splash water agent;

[0048] in:

[0049] The warp yarn is pigmented polyester / nylon solution-dyed fiber or core-spun stretch yarn.

[0050] The weft yarn is a pigmented polyester / nylon solution-dyed fiber and / or a core-spun stretch yarn. Based on this, when the weft yarn is selected from three different forms of pigmented polyester / nylon solution-dyed fiber, core-spun stretch yarn, or a combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn, the color fastness and dimensional stability can be improved, and when the combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn is used, the color fastness and dimensional stability effect is more significant.

[0051] It should be noted that the core-spun stretch yarn is composed of a polyolefin stretch yarn coated with a pigmented polyester / nylon solution-dyed fiber, and the weight percentage of the polyolefin stretch yarn in the first embodiment of the present application is 8wt%. The pigmented polyester / nylon solution-dyed fiber contains a colorant of 0.1wt% by weight, and the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5. The first matrix resin is a copolymer of ethylene and butene containing a first active group, and the molecular weight of the copolymer is less than 2000. The second matrix resin is a copolymer of ethylene and butene containing a second active group, and the molecular weight of the copolymer is less than 2000. Among them, the first active group is an isocyanate group. The second active group is an amino group.

[0052] The temperature of the Monfushi setting machine is controlled at 180°C, the speed is 40m / min, and the overfeed is 10%. In step 4, a silicon-based fluorine-free waterproof agent is used as a water-repellent agent in the Monfushi setting machine, and the temperature is controlled at 180°C, the speed is 30m / min, and the overfeed is 12%. Then, the heat setting is performed in an oven for 1-3 minutes, and the drying temperature is controlled at 100°C.

[0053] It should be mentioned that the colorant is carbon black coated with a chitosan composition. The chitosan composition accounts for 30wt% of the colorant. The particle size of the carbon black is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black and the chitosan composition. Among them, the chitosan composition is mixed with chitosan, a silane coupling agent, a multi-polymer of ethylene and butene, polyacrylate and / or polyacrylic acid vinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 13:3:2:2.5:0.6. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0054] like Figure 1 As shown, the warp yarn is the first yarn. The first yarn is polyester stock black DTY 75 / 72SD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is S-direction yarn. The weft yarn is the first yarn and the second yarn. The second yarn is polyester stock black ATY 340 / 144SD, and the density of the weft yarn is 164 strands / inch, the weft density is 144 strands / inch, and the gram weight is 275g / square meter. It should be noted that in step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1008, without sizing, and then combines them into a weaving shaft 1008*9; the loom adopts a double-nozzle machine, and hangs the first yarn on the first creel, and the second yarn on the second creel, and controls the speed of the loom to be 450rpm, and forms a first organization form with 8*12 coordinates to weave to obtain the first fabric, wherein the weft directions 1, 2, 3, 5, 7, 8, 9, 11 are the corresponding first yarns, and 4, 6, 10, 12 are the second yarns.

[0055] After testing, the warp elastic elongation of the fabric obtained in Example 1 is 19%, the weft elastic elongation is 22%, the weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 99%, and the warp elastic recovery is 99%; the color fastness of the fabric after 50 times washing at 75 degrees based on ENISO 20471:2013+A1:2016Clause5.3.3, ISO 105-C06:2010 is level 5, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016Clause 5.4 is 1.2%, and the weft dimensional stability is 1.0%.

[0056] Embodiment 2

[0057] A process for producing industrial washable workwear fabric comprises the following steps:

[0058] Step 1, warping, sizing and weaving: warp yarn is based on yarn specifications, above 70D is free of sizing, below 70D is sizing and waxing; weft yarn is sizing and then weaving; finally, warp yarn and weft yarn are woven;

[0059] Step 2, tension-free desizing: the fabric obtained by weaving treatment is dyed and finished by direct casting, which is used to stimulate the elasticity of the fabric so that it can fully shrink in the latter stage;

[0060] Step 3, mid-setting and drying: using Monforts setting machine;

[0061] Step 4: Splash water to finish: Use splash water agent;

[0062] in:

[0063] The warp yarn is pigmented polyester / nylon solution-dyed fiber or core-spun stretch yarn.

[0064] The weft yarn is a pigmented polyester / nylon solution-dyed fiber and / or a core-spun stretch yarn. Based on this, when the weft yarn is selected from three different forms of pigmented polyester / nylon solution-dyed fiber, core-spun stretch yarn, or a combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn, the color fastness and dimensional stability can be improved, and when the combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn is used, the color fastness and dimensional stability effect is more significant.

[0065] It should be noted that the core-spun stretch yarn is composed of a polyolefin stretch yarn coated with a pigmented polyester / nylon solution-dyed fiber, and the weight percentage of the polyolefin stretch yarn in the second embodiment of the present application is 16wt%. The pigmented polyester / nylon solution-dyed fiber contains a colorant of 2wt% by weight, and the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:1. The first matrix resin is a copolymer of ethylene and octene containing a first active group. The second matrix resin is a copolymer of ethylene and butene containing a second active group. Among them, the first active group is a silane coupling group. The second active group is an anhydride group.

[0066] The temperature of the Monfushi setting machine is controlled at 180°C, the speed is 40m / min, and the overfeed is 15%. In step 4, a silicon-based fluorine-free waterproof agent is used as a water-repellent agent in the Monfushi setting machine, and the temperature is controlled at 180°C, the speed is 30m / min, and the overfeed is 18%. Then, the heat setting is performed in an oven for 1-3 minutes, and the drying temperature is controlled at 100°C.

[0067] It should be mentioned that the colorant is an inorganic dye coated with a chitosan composition. The chitosan composition accounts for 40wt% of the colorant by weight. The particle size of the inorganic dye is 2-15μm, and the colorant is obtained by stirring and mixing the inorganic dye with the chitosan composition, polymerizing, filtering and drying. Wherein, the chitosan composition is composed of chitosan, a silane coupling agent, a multi-polymer of ethylene and butylene, polyacrylate and / or polyacrylic acid vinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 13:3:2:2.5:0.6.

[0068] like Figure 2As shown, the warp yarn in the second embodiment of the present application is the third yarn. The third yarn is nylon stock black DTY70 / 68FD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is Z-direction yarn. The weft yarns are the fourth yarn and the fifth yarn, the fourth yarn is nylon stock black DTY 70 / 68FD and polyolefin stretch yarn 42D, and the draft ratio of the core is 3.3, the twist is 800, and the twist direction is Z-direction yarn. The fifth yarn is double-strand nylon stock black DTY 140 / 136FD, and the density of the weft yarn is 158 strands / inch, the weft density is 156 strands / inch, and the gram weight is 250g / square meter. It should be noted that in step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1100, the yarns are sizing and waxed, and then they are combined into a weaving shaft 1100*8; the loom adopts a double-nozzle machine, and the fourth yarn is hung on the third creel, and the fifth yarn is hung on the fourth creel, the speed of the loom is controlled to be 450rpm, and the second fabric is woven in a second organizational form with 10*15 coordinates, wherein the weft directions 1, 2, 4, 5, 7, 8, 10, 11, 13, 14 are the corresponding fourth yarns, and 3, 6, 9, 12, 15 are the fifth yarns.

[0069] After testing, the warp elastic elongation of the fabric obtained in Example 2 is 18%, and the weft elastic elongation is 25%. The weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 98%, and the warp elastic recovery is 99%; the color fastness of the fabric after 50 times washing at 75 degrees based on ENISO 20471:2013+A1:2016Clause5.3.3, ISO 105-C06:2010 is level 5, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016Clause 5.4 is 1.2%, and the weft dimensional stability is 1.0%.

[0070] Embodiment 3

[0071] A process for producing industrial washable workwear fabric comprises the following steps:

[0072] Step 1, warping, sizing and weaving: warp yarn is based on yarn specifications, above 70D is free of sizing, below 70D is sizing and waxing; weft yarn is sizing and then weaving; finally, warp yarn and weft yarn are woven;

[0073] Step 2, tension-free desizing: the fabric obtained by weaving treatment is dyed and finished by direct casting, which is used to stimulate the elasticity of the fabric so that it can fully shrink in the latter stage;

[0074] Step 3, mid-setting and drying: using Monforts setting machine;

[0075] Step 4: Splash water to finish: Use splash water agent;

[0076] in:

[0077] The warp yarn is pigmented polyester / nylon solution-dyed fiber or core-spun stretch yarn.

[0078] The weft yarn is a pigmented polyester / nylon solution-dyed fiber and / or a core-spun stretch yarn. Based on this, when the weft yarn is selected from three different forms of pigmented polyester / nylon solution-dyed fiber, core-spun stretch yarn, or a combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn, the color fastness and dimensional stability can be improved, and when the combination of pigmented polyester / nylon solution-dyed fiber and core-spun stretch yarn is used, the color fastness and dimensional stability effect is more significant.

[0079] It should be noted that the core-spun stretch yarn is composed of a polyolefin stretch yarn coated with a pigmented polyester / nylon solution-dyed fiber, and the weight percentage of the polyolefin stretch yarn in the third embodiment of the present application is 24wt%. The pigmented polyester / nylon solution-dyed fiber contains 8wt% of a colorant by weight, and the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:2. The first matrix resin is a copolymer of ethylene and butene containing a first active group, and the second matrix resin is a copolymer of ethylene and octene containing a second active group. Among them, the first active group is an acrylamide group. The second active group is a hydroxyl group.

[0080] The temperature of the Monfushi setting machine is controlled at 180°C, the speed is 40m / min, and the overfeed is 15%. In step 4, a silicon-based fluorine-free waterproof agent is used as a water-repellent agent in the Monfushi setting machine, and the temperature is controlled at 180°C, the speed is 30m / min, and the overfeed is 20%. Then, the heat setting is performed in an oven for 1-3 minutes, and the drying temperature is controlled at 100°C.

[0081] It should be mentioned that the colorant is carbon black coated with a chitosan composition. The chitosan composition accounts for 25wt% of the colorant. The particle size of the carbon black is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black and the chitosan composition. Among them, the chitosan composition is composed of chitosan, a silane coupling agent, a binary or multi-polymer of ethylene and butene or octene, polyacrylate and / or polyacrylic acid vinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 14:2:5:2.5:0.3. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0082] like Figure 3As shown, the warp yarn is the sixth yarn. The sixth yarn is nylon stock gray DTY 140 / 96SD and polyolefin stretch yarn 105D, and the draft ratio of the core is 3.8, the twist is 700, and the twist direction is Z-direction yarn. The weft yarns are the sixth yarn and the seventh yarn. The seventh yarn is nylon stock gray ATY 160 / 96FD, and the density of the weft yarn is 106 strands / inch, the weft density is 144 strands / inch, and the gram weight is 268g / square meter. It should be noted that in step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1008, without sizing, and then combines them into a weaving shaft 1008*6; the loom adopts a double-nozzle machine, and hangs the sixth yarn on the fifth creel, and the seventh yarn on the sixth creel, and controls the speed of the loom to be 450rpm, and weaves a third fabric in a third organizational form with 6*12 coordinates, wherein the weft directions 1, 3, 5, 7, 9, 11 are the corresponding sixth yarns, and 2, 4, 6, 8, 10, 12 are the seventh yarns.

[0083] After testing, the warp elastic elongation of the fabric obtained in Example 3 is 18%, and the weft elastic elongation is 23%. The weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 98%, and the warp elastic recovery is 98%; based on ENISO 20471:2013+A1:2016Clause5.3.3, ISO 105-C06:2010, the color fastness of the fabric after 50 times washing at 75 degrees is level 5, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016Clause 5.4 is 1.1%, and the weft dimensional stability is 1.1%.

[0084] Embodiment 4

[0085] The difference between Example 4 and Example 1 is that the chitosan composition in Example 4 accounts for 10wt% of the colorant weight percentage. The particle size of carbon black is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black and the chitosan composition. Among them, the chitosan composition is mixed with chitosan, silane coupling agent, binary copolymer of ethylene and butene, polyacrylate, and methyl vinyl silicone oil in a weight ratio of 12:2:1:2:0.2. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0086] Embodiment 5

[0087] The difference between Example 5 and Example 1 is that the chitosan composition in Example 5 accounts for 50wt% of the colorant. The particle size of carbon black is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black and the chitosan composition. Among them, the chitosan composition is mixed with chitosan, silane coupling agent, multi-polymer of ethylene and octene, polyacryl vinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 16:4:5:3:0.8. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0088] Embodiment 6

[0089] The difference between Example 6 and Example 1 is that the pigment-type polyester / nylon solution-dyed fiber in Example 6 contains 2 wt % of colorant by weight.

[0090] After testing, the warp elastic elongation of the fabric obtained in Example 9 is 18%, and the weft elastic elongation is 21%. The weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 98%, and the warp elastic recovery is 98%; based on ENISO 20471:2013+A1:2016 Clause5.3.3, ISO 105-C06:2010, the color fastness of the fabric after 50 times washing at 75 degrees is level 5, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016 Clause 5.4 is 1.2%, and the weft dimensional stability is 1.2%.

[0091] Embodiment 7

[0092] The difference between Example 7 and Example 2 is that the colorant in Example 7 is an inorganic dye coated with a chitosan composition. The chitosan composition accounts for 10wt% of the colorant by weight. The particle size of the inorganic dye is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the inorganic dye and the chitosan composition. Among them, the chitosan composition is mixed with chitosan, a silane coupling agent, a binary copolymer of ethylene and butene, a polyacrylate, and methyl vinyl silicone oil in a weight ratio of 12:2:1:2:0.2. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0093] Embodiment 8

[0094] The difference between Example 8 and Example 2 is that the colorant in Example 8 is an inorganic dye coated with a chitosan composition. The chitosan composition accounts for 50wt% of the colorant by weight. The particle size of the inorganic dye is 2-15μm, and the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the inorganic dye and the chitosan composition. Among them, the chitosan composition is composed of chitosan, a silane coupling agent, a multi-polymer of ethylene and octene, polyacrylvinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 16:4:5:3:0.8. The carbon black is obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride.

[0095] Embodiment 9

[0096] The difference between Example 9 and Example 1 is that the warp yarn in Example 9 is polyester stock solution navy blue DTY 300 / 96SD. The weft yarn is polyester stock solution navy blue DTY 300 / 96SD and polyolefin stretch yarn 140D, and the draft ratio of the core is 3.8, the twist is 600, and the twist direction is S-direction yarn. A plain weave is adopted with a density of 66 strands / inch and a weft density of 56 strands / inch. It should be noted that in step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1223 whole shaft, free of sizing, and then combines them into a weaving shaft 1223*3. It is processed by a calendering process, in which the temperature is controlled at 140°C, the speed is 20m / min, and the pressure is 120N / mm, and then the transfer coating is performed based on the moisture-permeable base glue and the surface glue.

[0097] After testing, the weft elastic elongation of the fabric obtained in Example 9 is 18%, the weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 98%, the color fastness of the fabric after 50 washes at 75 degrees based on EN ISO 20471:2013+A1:2016 Clause 5.3.3, ISO105-C06:2010 is level 4-5, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016 Clause 5.4 is 1.3%, and the weft dimensional stability is 1.1%.

[0098] Embodiment 10

[0099] The difference between Example 10 and Example 1 is that the warp yarn in Example 10 is polyester stock black DTY 75 / 72SD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is S-direction yarn. The weft yarn is polyester stock black DTY 75 / 72SD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is S-direction yarn.

[0100] The plain weave is used with a density of 126 strands / inch and a weft density of 112 strands / inch. It should be noted that in step 1, the warping machine evenly arranges the warp yarns and forms a whole axis 1052, without sizing, and then forms a weaving axis 1052*7. And it is bonded and finished. The bonding and finishing is bonded by hot melt adhesive engraving roller lamination process, and the temperature is controlled at 40℃ for aging for 24 hours.

[0101] After testing, the weft elastic elongation of the fabric obtained in Example 10 is 18%, the weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 98%, the color fastness of the fabric after 50 washes at 75 degrees based on EN ISO 20471:2013+A1:2016 Clause 5.3.3, ISO105-C06:2010 is level 4-5, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016 Clause 5.4 is 1.4%, and the weft dimensional stability is 1.1%.

[0102] Embodiment 10

[0103] The difference between the eleventh embodiment and the first embodiment is that the temperature of the Monfushi setting machine in the eleventh embodiment is controlled at 180°C, the speed is 40m / min, and the overfeed is 3%. In step 4, a silicon-based fluorine-free waterproof agent is used as a water-splashing agent in the Monfushi setting machine, and the temperature is controlled at 180°C, the speed is 30m / min, and the overfeed is 3%. Then, the oven is used for heat setting for 1-3 minutes, and the drying temperature is controlled at 100°C.

[0104] Embodiment 10

[0105] The difference between the eleventh embodiment and the first embodiment is that the temperature of the Monfushi setting machine in the eleventh embodiment is controlled at 180°C, the speed is 40m / min, and the overfeed is 22%. In step 4, a silicon-based fluorine-free waterproof agent is used as a water-splashing agent in the Monfushi setting machine, and the temperature is controlled at 180°C, the speed is 30m / min, and the overfeed is 22%. Then, the setting is performed in an oven for 1-3 minutes, and the drying temperature is controlled at 100°C.

[0106] Comparative Example 1

[0107] The difference between Comparative Example 1 and Example 1 is that the polyolefin stretch yarn in Comparative Example 1 does not contain active functional groups.

[0108] After testing, the warp elastic elongation of the fabric obtained in Comparative Example 1 is 22%, and the weft elastic elongation is 24%. The weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 93%, and the warp elastic recovery is 91%. The color fastness of the fabric after 50 times washing at 75 degrees based on ENISO 20471:2013+A1:2016 Clause5.3.3, ISO 105-C06:2010 is level 4-5, and the radial dimensional stability in the dimensional stability obtained based on EN ISO 20471:2013+A1:2016 Clause 5.4 is 4.5%, and the weft dimensional stability is 3.7%.

[0109] Comparative Example 2

[0110] The difference between Comparative Example 2 and Example 1 is that the colorant in Comparative Example 2 does not contain the chitosan composition.

[0111] After testing, the warp elastic elongation of the fabric obtained in Comparative Example 2 is 9%, and the weft elastic elongation is 11%. The weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is 85%, and the warp elastic recovery is 87%; based on ENISO 20471:2013+A1:2016 Clause5.3.3, ISO 105-C06:2010, the color fastness of the fabric after 50 times washing at 75 degrees is level 3, and the radial dimensional stability of the dimensional stability obtained based on EN ISO 20471:2013+A1:2016 Clause 5.4 is 8.2%, and the weft dimensional stability is 7.8%.

[0112] It can be seen that by using the chitosan composition to coat the carbon black obtained by grafting and modifying hydroxymethyl carbon black with maleic anhydride, the adhesion stability of the carbon black can be improved and the negative impact of the carbon black on the mechanical properties of the fabric can be avoided. For inorganic dyes, the use of the chitosan composition for coating and knitting with polyolefin stretch yarns with active functional groups will significantly improve the mechanical properties of the fabric, and cooperate with the weaving combination of two new types of warp and weft yarns, so that the fabric has the effect of high color fastness and high dimensional stability.

[0113] In summary, the present application provides a process for producing industrial water-washing resistant workwear fabrics, which has the effect of significantly improving the color fastness and dimensional stability of the fabrics; the weft elastic elongation is more than 18%, the weft elastic recovery of the fabric obtained based on FZ / T01062-1999 is more than 97%, the color fastness of the fabric after 50 washes at 75 degrees based on EN ISO20471:2013+A1:2016Clause 5.3.3, ISO 105-C06:2010 is more than level 4, and the dimensional stability is within ±1.5% based on EN ISO 20471:2013+A1:2016Clause5.4.

[0114] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, or devices.

[0115] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0116] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A process for producing industrial washable workwear fabric, characterized in that: The steps include: Step 1, warping, sizing and weaving: warp yarn is based on yarn specifications, above 70D is free of sizing, below 70D is sizing and waxing; weft yarn is sizing and then weaving; finally, warp yarn and weft yarn are woven; Step 2, tension-free desizing: the fabric obtained by weaving treatment is dyed and finished by direct casting, which is used to stimulate the elasticity of the fabric so that it can fully shrink in the latter stage; Step 3, mid-setting and drying: using Monforts setting machine; Step 4: Splash water to finish: Use splash water agent; Wherein, the warp yarn is a pigmented polyester / nylon solution-dyed fiber or a core-spun stretch yarn; the weft yarn is a pigmented polyester / nylon solution-dyed fiber and / or a core-spun stretch yarn; the core-spun stretch yarn is composed of a pigmented polyester / nylon solution-dyed fiber coated with a polyolefin stretch yarn, and the weight percentage of the polyolefin stretch yarn in the core-spun stretch yarn is 8-24wt%; the pigmented polyester / nylon solution-dyed fiber contains a colorant in an amount of 0.1-8wt% by weight; the polyolefin stretch yarn is obtained by melt spinning after mixing a first matrix resin and a second matrix resin in a mass ratio of 1:0.5-2.

2. The process for producing industrial washable workwear fabric according to claim 1, characterized in that: The method also includes the steps of calendering, coating or laminating the fabric after water splashing finishing; the calendering is carried out through the calendering process, controlling the temperature to 140°C, the speed to 20m / min, and the pressure to 120N / mm, and then transferring the coating based on the moisture-permeable base glue and the surface glue; the laminating finishing is carried out by laminating with a hot melt adhesive engraving roller, and controlling the temperature to 40-60°C for 24 hours.

3. The process for producing industrial washable workwear fabric according to claim 1, characterized in that: The first matrix resin is a copolymer of ethylene and butene or octene containing a first active group, and the second matrix resin is a copolymer of ethylene and butene or octene containing a second active group; wherein the first active group is an isocyanate group, an acrylamide group, a silane coupling group, an acyl chloride group or a sulfonic acid group; and the second active group is an amino group, a hydroxyl group, a cyano group, an epoxy group, a thiol group or an anhydride group.

4. The process for producing industrial washable workwear fabric according to claim 1, characterized in that: The colorant is carbon black or inorganic dye coated with a chitosan composition; the chitosan composition accounts for 10-50wt% of the colorant; the particle size of the carbon black or inorganic dye is 2-15μm; the colorant is obtained by stirring, mixing, polymerizing, filtering and drying the carbon black or inorganic dye and the chitosan composition.

5. The process for producing industrial washable workwear fabric according to claim 5, characterized in that: The chitosan composition is prepared by mixing chitosan, silane coupling agent, binary or multi-polymer of ethylene and butene or octene, polyacrylate and / or polyacrylic acid vinyl alcohol ester, and methyl vinyl silicone oil in a weight ratio of 12-16:2-4:1-5:2-3:0.2-0.

8.

6. The process for producing industrial washable workwear fabric according to claim 5, characterized in that: The carbon black is obtained by grafting hydroxymethyl carbon black with maleic anhydride.

7. The process for producing industrial washable workwear fabric according to claim 1, characterized in that: The warp yarn is the first yarn, the first yarn is polyester stock black DTY 75 / 72SD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is S-direction yarn; the weft yarn is the first yarn and the second yarn, the second yarn is polyester stock black ATY 340 / 144SD, and the density of the weft yarn is 164 strands / inch, the weft density is 144 strands / inch, and the gram weight is 275g / square meter; in step 1, the warping machine arranges the warp yarn evenly and forms a whole shaft 1008 whole shaft, without sizing, and then forms a weaving shaft 1008*9; the loom adopts a double-nozzle machine, and hangs the first yarn on the first creel, and hangs the second yarn on the second creel, controls the rotation speed of the loom to 450rpm, and forms a first organization form with 8*12 coordinates to weave to obtain a first fabric, wherein the weft directions 1, 2, 3, 5, 7, 8, 9, 11 are the corresponding first yarns, and 4, 6, 10, 12 are the second yarns.

8. The process for producing industrial washable workwear fabric according to claim 1, characterized in that: The warp yarn is the third yarn, the third yarn is nylon liquid black DTY 70 / 68FD and polyolefin stretch yarn 75D, and the draft ratio of the core is 3.5, the twist is 800, and the twist direction is Z-direction yarn; the weft yarn is the fourth yarn and the fifth yarn, the fourth yarn is nylon liquid black DTY 70 / 68FD and polyolefin stretch yarn 42D, and the draft ratio of the core is 3.3, the twist is 800, and the twist direction is Z-direction yarn; the fifth yarn is double-strand nylon liquid black DTY 140 / 136FD, and the density of the weft yarn is 158 strands / inch, the weft density is 156 strands / inch, and the gram weight is 250g / square meter; in step 1, the warping machine arranges the warp yarn evenly and forms a whole shaft of 1100 whole shafts, the sizing yarn is waxed, and then combined into a weaving shaft of 1100*8; the loom adopts a double-nozzle machine, and the fourth yarn is hung on the third creel, and the fifth yarn is hung on the fourth creel, the speed of the loom is controlled to be 450rpm, and the second fabric is woven in a second organizational form with 10*15 coordinates, wherein the weft directions 1, 2, 4, 5, 7, 8, 10, 11, 13, 14 are the corresponding fourth yarns, and 3, 6, 9, 12, 15 are the fifth yarns.

9. The process for producing industrial washable workwear fabric according to claim 1, characterized in that: The warp yarn is the sixth yarn, the sixth yarn is nylon stock gray DTY 140 / 96SD and polyolefin stretch yarn 105D, and the draft ratio of the core is 3.8, the twist is 700, and the twist direction is Z-direction yarn; the weft yarn is the sixth yarn and the seventh yarn, the seventh yarn is nylon stock gray ATY 160 / 96FD, and the density of the weft yarn is 106 yarns / inch, the weft density is 144 yarns / inch, and the gram weight is 268g / square meter; in step 1, the warping machine arranges the warp yarns evenly and forms a whole shaft 1008 whole shaft, without sizing, and then forms a weaving shaft 1008*6; the loom adopts a double-nozzle machine, and hangs the sixth yarn on the fifth creel, and hangs the seventh yarn on the sixth creel, controls the speed of the loom to 450rpm, and forms a third organization form with 6*12 coordinates to weave to obtain a third fabric, wherein the weft directions 1, 3, 5, 7, 9, 11 are the corresponding sixth yarns, and 2, 4, 6, 8, 10, 12 are the seventh yarns.

10. A process for producing industrial washable workwear fabric according to any one of claims 7, 8 and 9, characterized in that: The temperature of the Monforts setting machine is controlled at 180°C, the speed is 40m / min, and the overfeed is 3%-22%; And in step 4, a silicon-based fluorine-free waterproof agent is used as a water-repellent in a Monforts setting machine, the temperature is controlled at 180°C, the speed is 30m / min, the overfeed is 3%-22%, and then the heat setting is carried out in an oven for 1-3min, and the drying temperature is controlled at 100°C.

Citation Information

Patent Citations

  • Manufacturing process for low-temperature shaped elastic coating yarn

    CN101200825A

  • Spun-dyed black polyamide yarn, false-twisted yarn, covered elastomer yarn, and leg knit

    CN104220653A

  • Making process of high-fastness polyamide-polyester interwoven fabric

    CN106757673A

  • Chitosan derivative used as dispersing agent and application thereof in fabric printing and dyeing

    CN106986953A

  • Carbon black color paste and preparation method and application thereof

    CN111826027A