Preparation method and application of protein fiber immobilized zirconium-based activated carbon hybrid membrane
By solidifying the zirconium-based activated carbon on the protein fibers, an efficient membrane was prepared, which solved the problem of sulfadiazine antibiotic treatment in water, achieved efficient adsorption and removal, reduced environmental pollution, and provided a green water treatment solution.
Patent Information
- Application Number
- CN202410974493.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to effectively treat sulfadiazine antibiotics in water. The catalytic area of traditional nanoads is limited, the adsorption efficiency is low, and the removal effect of specific pollutants is poor, resulting in environmental pollution.
The preparation method of protein fiber-supported zirconium-based activated carbon hybrid membrane was adopted to form ZrO2 particles through the reaction of whey protein and ZrOCl2·7H2O. Combined with activated carbon, a membrane with high-efficiency adsorption capacity was prepared to remove sulfadiazine antibiotics.
It significantly improves the adsorption efficiency of sulfadiazine antibiotics, reduces secondary pollution in the environment, provides an efficient and green water treatment technology, and overcomes the limitations of traditional nano adsorbents.
Smart Images

Figure CN119083154A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment material preparation, and specifically relates to a preparation method and application of a protein fiber-immobilized zirconium-based activated carbon hybrid membrane. Background Art
[0002] Antibiotics are new pollutants in water bodies, among which sulfonamide antibiotics are one of the most common and commonly used antibiotics. The increase of antibiotics in the environment will lead to bacterial resistance, inhibit cell growth and have a negative impact on the aquatic ecosystem. Due to the chemical properties of sulfonamide antibiotics, most of them will be discharged in the form of metabolites or animal excrement in different ways all year round and accumulated in surface water, groundwater and soil. They have become the most frequently detected type of antibiotics in the environment. Sulfadiazine is stable in nature in water, and it is difficult to effectively treat sulfadiazine antibiotics in water with conventional water treatment processes in sewage treatment plants. Therefore, finding an efficient and green new treatment technology and method is of practical significance for solving the problem of sulfadiazine antibiotics in water bodies.
[0003] At present, the commonly used methods for removing antibiotics from water bodies at home and abroad include physicochemical method, biological method, electrochemical method and membrane filtration method; among them, the physicochemical method is difficult to use on a large scale due to its high regeneration cost and excessive energy consumption; antibiotics are toxic to microorganisms, so the removal effect of microorganisms that have not been specially domesticated is very limited; the electrochemical method requires a large amount of electricity to treat low-level pollutants, resulting in high treatment costs and is difficult to use on a large scale.
[0004] Membrane technology is widely used in environmental water treatment due to its significant removal effect and strong renewability. However, the high cost of membrane component equipment and operation makes it difficult to remove specific organic matter on a large scale, which results in certain limitations. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a protein fiber-immobilized zirconium-based activated carbon hybrid membrane.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a protein fiber-immobilized zirconium-based activated carbon hybrid membrane, comprising:
[0009] Dissolving whey protein monomer in deionized water to prepare a whey protein solution;
[0010] The pH value of the whey protein solution is adjusted to 2, and the temperature is raised and stirred to obtain a whey protein deformation solution;
[0011] After standing, ZrOCl2·7H2O was added and the solution was adjusted to pH 3.5-4.0. 4+ Oxidized into ZrO2 particles, which were immobilized on the protein-like fibers to obtain solution 1;
[0012] The activated carbon is dissolved in deionized water, and the activated carbon is evenly dispersed in the solution by ultrasonic treatment to prepare solution 2;
[0013] Mix solution 1 and solution 2 thoroughly;
[0014] The mixed liquid is evenly distributed on the fiber membrane. After suction filtration and observation that there is no water on the membrane surface, the suction filtration is stopped and the membrane is dried to obtain a zirconium-based adsorption membrane constructed with protein fibers.
[0015] As a preferred embodiment of the preparation method of the present invention, the whey protein solution is prepared, wherein the ratio of whey protein monomer to deionized water is 2-4 g: 180-300 mL.
[0016] As a preferred embodiment of the preparation method of the present invention, the whey protein deformation solution is prepared by heating and stirring, wherein the temperature is raised to 80-90° C., the stirring speed is 300-400 rpm, and the stirring time is 4-5 hours.
[0017] As a preferred embodiment of the preparation method of the present invention, the pH of the whey protein solution is adjusted to 2, wherein the adjusted solution comprises a 1M HCl solution.
[0018] As a preferred embodiment of the preparation method of the present invention, 4 g ZrOCl2·7H2O is added to 20 mL of whey protein deformation solution and stirred, and the pH of the solution after stirring is adjusted to 3.5-4.0. The generation of white precipitate indicates that ZrOCl2·7H2O is 4+ ZrO2 particles were oxidized and successfully immobilized on protein fibers, wherein the adjusted solution included 1 M NaOH solution.
[0019] As a preferred embodiment of the preparation method of the present invention, the ultrasonic treatment makes the activated carbon uniformly dispersed in deionized water with a mass fraction of 10wt%, wherein the temperature of the ultrasonic treatment is 25°C, the time is 30min, and the power is 180W.
[0020] As a preferred embodiment of the preparation method of the present invention, solution 1 and solution 2 are fully mixed for 30 minutes.
[0021] As a preferred embodiment of the preparation method of the present invention, the mixed solution is filtered in a filtration device SCJ-10, the filtration time is 3 minutes, the negative pressure is 0.08 MPa, and the flow rate is 10 L / min.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide a protein fiber-immobilized zirconium-based activated carbon hybrid membrane.
[0023] Another object of the present invention is to overcome the deficiencies in the prior art and provide a protein fiber-immobilized zirconium-based activated carbon hybrid membrane for use in removing sulfadiazine.
[0024] Beneficial effects of the present invention:
[0025] (1) The present invention aims to solve the problem of low adsorption efficiency of traditional nano-adsorbents due to their limited catalytic area and adsorption efficiency being limited by the nano-adsorbent material itself. By immobilizing Zr clusters on a protein-like fiber template, a protein fiber-constructed zirconium-based activated carbon composite adsorption membrane is prepared. Compared with a single nano-adsorbent, the adsorption efficiency of sulfadiazine by the Zr clusters immobilized on the protein-like fiber is significantly improved.
[0026] (2) In view of the shortcoming that traditional nanocatalysts cannot effectively remove single pollutants, the present invention can specifically adsorb sulfadiazine antibiotics by immobilizing Zr clusters, thereby increasing the adsorption effect of the adsorption membrane on sulfadiazine antibiotics; the protein-like fibers have a certain viscosity that can make the activated carbon fully adhere together, effectively solving the secondary pollution caused by traditional nanoadsorbents to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0028] Figure 1 This is an electronic scanning image of the zirconium-based activated carbon composite adsorption film constructed by the protein fiber prepared in Example 1 of the present invention.
[0029] Figure 2 This is a diagram showing the effect of the membrane in the embodiment of the present invention in removing antibiotics under different pH conditions.
[0030] Figure 3This is a comparison diagram of the adsorption capacity of the membrane at different concentrations in the embodiments of the present invention.
[0031] Figure 4 The figure is a comparison chart of the adsorption capacity of the membranes prepared in the comparative examples of the present invention at different concentrations. DETAILED DESCRIPTION
[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0033] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0034] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0035] The particle size of the activated carbon in the embodiment of the present invention is less than 30 nm, and it is from Sinopharm Chemical Reagent Co., Ltd.; other raw materials are all common commercially available products.
[0036] Example 1
[0037] The preparation of protein fiber-constructed zirconium-based activated carbon composite adsorption membrane specifically includes the following steps:
[0038] (1) 3 g of whey protein monomer was added to 280 mL of deionized water to fully dissolve the whey protein monomer in the deionized water, and the pH of the solution was adjusted to 2.03 using 1 M HCl solution.
[0039] (2) Stir thoroughly on a magnetic stirrer at 90°C and 740 rpm for 8 h to allow the whey protein monomers to form protein-like fibers.
[0040] (3) 4 g ZrOCl2·7H2O solid was completely dissolved in 20 mL of the solution prepared in step (2) above, and mixed on a mixer with a power of 60 W for 30 min to make it fully and evenly dissolved in the solution. The mass fraction of the obtained solution was 2 wt%.
[0041] (4) Add 1 M NaOH solution to the above step (3), adjust the pH of the solution to 3.5-4.0, and observe the appearance of white precipitate in the solution, indicating that the ZrO2 nanoparticles have been successfully immobilized on the protein-like fibers. The obtained solution is numbered as solution 1.
[0042] (5) Dissolve 2 g of activated carbon in 20 mL of deionized water, and fully mix the activated carbon dispersion solution on a mixer with a power of 60 W to make the activated carbon evenly dispersed in the solution to obtain an activated carbon dispersion solution with a mass fraction of 10 wt%. The obtained solution is numbered as solution 2.
[0043] (6) Immediately mix 3 mL of solution 1 and 3 mL of solution 2 on a 60 W mixer.
[0044] (7) The mixed solution in the above step (6) was subjected to ultrasonic treatment at 90° C. for 1 h to remove bubbles in the mixed solution.
[0045] (8) 3 mL of the mixed solution in step (7) was extracted onto a fiber membrane with a pore size of 0.22 μm to make it evenly distributed, and then filtered using a SCJ-10 vacuum filtration device with a filtration time of 3 min, a negative pressure of 0.08 MPa, and a flow rate of 10 L / min. The filtration was stopped after observing that there was no moisture on the membrane surface. The protein fiber-constructed zirconium-based activated carbon composite adsorption membrane was successfully formed on the fiber membrane.
[0046] (9) The prepared membrane was dried at 25°C for 24 hours to complete the preparation of the protein fiber constructed zirconium-based activated carbon composite adsorption membrane.
[0047] Electron scanning images of protein fiber-constructed zirconium-based activated carbon composite adsorption membranes are shown in Figure 1 .
[0048] Example 2
[0049] (1) Protein fiber construction The preparation steps of nanocatalysts were the same as those in Example 1, except that in step 1, 4 g of whey protein monomer was added to 380 mL of deionized water, the pH of the solution was adjusted to 2.06, and the total volume of the solution was 400 mL.
[0050] (2) Stir thoroughly on a magnetic stirrer at 90°C and 740 rpm for 8 h to allow the whey protein monomers to form protein-like fibers.
[0051] (3) 4 g ZrOCl2·7H2O solid was completely dissolved in 20 mL of the solution prepared in step (2) above, and mixed on a mixer with a power of 60 W for 30 min to make it fully and evenly dissolved in the solution. The mass fraction of the obtained solution was 2 wt%.
[0052] (4) Add 1 M NaOH solution to the above step (3), adjust the pH of the solution to 3.5-4.0, and observe the appearance of white precipitate in the solution, indicating that the ZrO2 nanoparticles have been successfully immobilized on the protein-like fibers. The obtained solution is numbered as solution 1.
[0053] (5) Dissolve 2 g of activated carbon in 20 mL of deionized water, and fully mix the activated carbon dispersion solution on a mixer with a power of 60 W to make the activated carbon evenly dispersed in the solution to obtain an activated carbon dispersion solution with a mass fraction of 10 wt%. The obtained solution is numbered as solution 2.
[0054] (6) Immediately mix 3 mL of solution 1 and 3 mL of solution 2 on a 60 W mixer.
[0055] (7) The mixed solution in the above step (6) was subjected to ultrasonic treatment at 90° C. for 1 h to remove bubbles in the mixed solution.
[0056] (8) 3 mL of the mixed solution in step (7) was extracted onto a fiber membrane with a pore size of 0.22 μm to make it evenly distributed, and then filtered using a SCJ-10 vacuum filtration device with a filtration time of 3 min, a negative pressure of 0.08 MPa, and a flow rate of 10 L / min. The filtration was stopped after observing that there was no moisture on the membrane surface. The protein fiber-constructed zirconium-based activated carbon composite adsorption membrane was successfully formed on the fiber membrane.
[0057] (9) The prepared membrane was dried at 25°C for 24 hours to complete the preparation of the protein fiber constructed zirconium-based activated carbon composite adsorption membrane.
[0058] Example 3
[0059] (1) Protein fiber construction The preparation steps of nanocatalysts were the same as those in Example 1, except that in step 1, 2 g of whey protein monomer was added to 180 mL of deionized water, the pH of the solution was adjusted to 2, and the final total volume of the solution was 200 mL.
[0060] (2) Stir thoroughly on a magnetic stirrer at 90°C and 740 rpm for 8 h to allow the albumin monomers to form protein-like fibers.
[0061] (3) 4 g ZrOCl2·7H2O solid was completely dissolved in 20 mL of the solution prepared in step (2) above, and mixed on a mixer with a power of 60 W for 30 min to make it fully and evenly dissolved in the solution. The mass fraction of the obtained solution was 2 wt%.
[0062] (4) Add 1 M NaOH solution to the above step (3), adjust the pH of the solution to 3.5-4.0, and observe the appearance of white precipitate in the solution, indicating that the ZrO2 nanoparticles have been successfully immobilized on the protein-like fibers. The obtained solution is numbered as solution 1.
[0063] (5) Dissolve 2 g of activated carbon in 18 mL of deionized water, and fully mix the activated carbon dispersion solution on a mixer with a power of 60 W to make the activated carbon evenly dispersed in the solution to obtain an activated carbon dispersion solution with a mass fraction of 10 wt%. The obtained solution is numbered as solution 2.
[0064] (6) Immediately mix 3 mL of solution 1 and 3 mL of solution 2 on a 60 W mixer.
[0065] (7) The mixed solution in the above step (6) was subjected to ultrasonic treatment at 90° C. for 1 h to remove bubbles in the mixed solution.
[0066] (8) 3 mL of the mixed solution in step (7) was extracted onto a fiber membrane with a pore size of 0.22 μm to make it evenly distributed, and then filtered using a SCJ-10 vacuum filtration device with a filtration time of 3 min, a negative pressure of 0.08 MPa, and a flow rate of 10 L / min. The filtration was stopped after observing that there was no moisture on the membrane surface. The protein fiber-constructed zirconium-based activated carbon composite adsorption membrane was successfully formed on the fiber membrane.
[0067] (9) The prepared membrane was dried at 25°C for 24 hours to complete the preparation of the protein fiber constructed zirconium-based activated carbon composite adsorption membrane.
[0068] Example 4
[0069] The pH gradient was adjusted using 1M HCl and NaOH solutions. The test gradient was 1. At a concentration of 150 mg / L sulfadiazine, the filtration volume was 100 mL, the filtration time was 1 min, the test vacuum pressure was 0.068 MPa, and the vacuum filter was SCJ-10. The membrane under different pH conditions was used to remove antibiotics.
[0070] The protein fiber constructed zirconium-based activated carbon composite adsorption membrane in Example 1 was used to test the adsorption performance of sulfadiazine under different pH conditions. At a sulfadiazine concentration of 150 mg / L, the adsorption amount of sulfadiazine by the protein fiber constructed zirconium-based activated carbon composite adsorption membrane was tested under pH conditions of 2 to 9. The adsorption was tested using an ultraviolet spectrophotometer, and the equilibrium adsorption amount was calculated using the formula qe=V×(C0-C) / W(mg / g);
[0071] In the formula: V is the volume of wastewater, L; W is the mass of adsorbent, g; C0 is the concentration of adsorbate in raw water, mg / L; C is the concentration of adsorbate remaining in water at adsorption equilibrium, mg / L.
[0072] Results Figure 2 ,Depend on Figure 2It can be seen that with the increase of pH, the adsorption amount of sulfadiazine first increases and then decreases, and the adsorption amount is the largest when pH = 7.8.
[0073] Application Example 1
[0074] The zirconium-based activated carbon composite adsorption membrane constructed with the protein fiber in Example 1 was used to analyze the removal performance of sulfadiazine antibiotics:
[0075] The membrane was added to 1000 ml of sulfadiazine solution with concentrations of 10, 20, 40, 60, 80, 100, 120, 140, 160, and 180 mg / L;
[0076] The above concentrations were adsorbed on the zirconium-based activated carbon composite adsorption membrane constructed by protein fibers. The membrane was placed in a sulfadiazine solution with a volume of 1000 ml and a pH of 7.8. The adsorption was continued at 150 rpm for 20 minutes. The residual concentration of the solution was tested under an ultraviolet spectrophotometer. The adsorption amount of sulfadiazine by the zirconium-based activated carbon composite adsorption membrane constructed by protein fibers was calculated. The equilibrium adsorption amount (Qe) = (Co-Ce) * V / m, where Co is the initial concentration of the adsorbate, Ce is the concentration at equilibrium, V is the volume of the adsorbate, and m is the mass of the adsorbent.
[0077] The adsorption performance of the membrane was tested and the results are shown in Figure 3 Sample 1 in.
[0078] Application Example 2
[0079] The membrane was prepared by the method of preparing protein fiber to construct zirconium-based activated carbon composite adsorption membrane in Example 2, and the removal effect of the membrane on sulfadiazine in water was tested at the maximum adsorption amount;
[0080] The membrane was added to 1000 ml of sulfadiazine solution with concentrations of 10, 20, 40, 60, 80, 100, 120, 140, 160, and 180 mg / L, pH = 7.8, and shaken at 150 rpm for 30 min. The residual sulfadiazine concentration was determined by UV-visible light; the results are shown in Figure 3 Sample 2.
[0081] The absorbance at the initial concentration of sulfadiazine was tested. After the membrane material was shaken continuously for 30 minutes to fully adsorb the sulfadiazine solution, the absorbance of the adsorbed solution was tested again. The equilibrium adsorption amount (Qe) was calculated using the formula (Co-Ce)*V / m, where Co is the initial concentration of the adsorbate, Ce is the concentration at equilibrium, V is the volume of the adsorbate, and m is the mass of the adsorbent.
[0082] Application Example 3
[0083] The membrane was prepared by the method of preparing protein fiber to construct zirconium-based activated carbon composite adsorption membrane in Example 3, and the removal effect of the membrane on sulfadiazine in water was tested when the initial concentration of sulfadiazine was set to the same as that in Application Example 2 at the maximum adsorption amount;
[0084] Test the absorbance at the initial concentration of sulfadiazine, shake it continuously for 30 minutes, and then test the absorbance after filtration. Use the formula in Application Example 2 to calculate the corresponding adsorption capacity. The results are shown in Figure 3 Sample 3.
[0085] Comparative Example 1
[0086] The membrane was prepared by the method of preparing protein fiber to construct zirconium-based activated carbon composite adsorption membrane in Example 1, except that no ZrOCl2·7H2O solid was added in step (3). The maximum adsorption capacity of the membrane prepared in this way and the removal effect of the membrane on sulfadiazine solution in water were tested.
[0087] The membrane prepared by this method was added to 1000 ml of sulfadiazine solution with concentrations of 10, 20, 40, 60, 80, 100, 120, 140, 160, and 180 mg / L, pH = 7.8, and shaken at 150 rpm for 30 minutes. The residual sulfadiazine concentration was determined by UV-visible light; the results are shown in Figure 4 Medium sample 5;
[0088] Note: The results of the experiment were obtained by repeating the experiment in Application Example 1. Figure 4 Sample 4.
[0089] Depend on Figure 4 It can be seen from sample 4 and sample 5 that the removal effects are in sharp contrast, indicating that the immobilized Zr causes a significant change in the properties of the membrane.
[0090] Comparative Example 2
[0091] The membrane was prepared by the method of preparing protein fiber to construct zirconium-based activated carbon composite adsorption membrane in Example 1, except that no whey protein monomer was added in step (1) and no ZrOCl2·7H2O solid was added in step (3). The maximum adsorption capacity of the membrane prepared in this way and the removal effect of the membrane on sulfadiazine solution in water were tested.
[0092] The membrane prepared by this method was added into 1000 ml of sulfadiazine solution with concentrations of 10, 20, 40, 60, 80, 100, 120, 140, 160, 180 mg / L, pH = 7.8, and shaken at 150 rpm for 30 min. The residual sulfadiazine concentration was determined by UV-visible light.
[0093] Results Figure 4 Sample 6, Figure 4Comparing Sample 6 with Sample 5, it can be seen that the construction of protein fibers on the membrane has a certain improvement effect on the properties of the membrane.
[0094] Comparative Example 3
[0095] The membrane was prepared by the method of preparing protein fiber to construct zirconium-based activated carbon composite adsorption membrane in Example 1, except that step (3) was adjusted to add 4 g Zr(SO4)2 solid, and the other conditions were the same as in Example 1.
[0096] The maximum adsorption capacity of the membrane prepared in this way and the removal effect of the membrane on sulfadiazine solution in water were tested.
[0097] The membrane prepared by this method was added into 1000 ml of sulfadiazine solution with concentrations of 10, 20, 40, 60, 80, 100, 120, 140, 160, 180 mg / L, pH = 7.8, and shaken at 150 rpm for 30 min. The residual sulfadiazine concentration was determined by UV-visible light.
[0098] Results Figure 4 Sample 7, Figure 4 Comparing sample 4 with sample 7, it can be seen that the metal clusters supported by ZrOCl2·7H2O solid are significantly better than the metal clusters constructed by Zr(SO4)2 solid.
[0099] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing a protein fiber-immobilized zirconium-based activated carbon hybrid membrane, characterized in that: include, Dissolving whey protein monomer in deionized water to prepare a whey protein solution; The pH value of the whey protein solution is adjusted to 2, and the temperature is raised and stirred to obtain a whey protein deformation solution; After standing, ZrOCl2·7H2O was added and the solution was adjusted to pH 3.5-4.
0. 4+ Oxidized into ZrO2 particles, which were immobilized on the protein-like fibers to obtain solution 1; The activated carbon is dissolved in deionized water, and the activated carbon is evenly dispersed in the solution by ultrasonic treatment to prepare solution 2; Mix solution 1 and solution 2 thoroughly; The mixed liquid is evenly distributed on the fiber membrane. After suction filtration and observation that there is no water on the membrane surface, the suction filtration is stopped and the membrane is dried to obtain a zirconium-based adsorption membrane constructed with protein fibers.
2. The preparation method according to claim 1, characterized in that: The prepared whey protein solution comprises whey protein monomer and deionized water in a ratio of 2-4 g to 180-300 mL.
3. The preparation method according to claim 1 or 2, characterized in that: The whey protein deformation solution is prepared by heating and stirring, wherein the temperature is raised to 80-90° C., the stirring speed is 300-400 rpm, and the stirring time is 4-5 hours.
4. The preparation method according to claim 1 or 2, characterized in that: The pH value of the whey protein solution is adjusted to 2, wherein the adjusted solution comprises 1M HCl solution.
5. The preparation method according to claim 1, characterized in that: 4 g ZrOCl2·7H2O was added to 20 mL of whey protein deformation solution and stirred, and the pH of the solution after stirring was adjusted to 3.5-4.
0. White precipitate was observed, indicating that ZrOCl2·7H2O 4+ ZrO2 particles were oxidized and successfully immobilized on protein fibers, wherein the adjusted solution included 1 M NaOH solution.
6. The preparation method according to claim 1, characterized in that: The ultrasonic treatment makes the activated carbon uniformly dispersed in deionized water with a mass fraction of 10wt%, wherein the temperature of the ultrasonic treatment is 25°C, the time is 30min, and the power is 180W.
7. The preparation method according to claim 1, characterized in that: The solution 1 and the solution 2 were fully mixed, and the mixing time was 30 minutes.
8. The preparation method according to claim 1, characterized in that: The mixed solution was filtered in a filtration device SCJ-10, with a filtration time of 3 min, a negative pressure of 0.08 MPa, and a flow rate of 10 L / min.
9. The protein fiber-immobilized zirconium-based activated carbon hybrid membrane prepared by the preparation method described in any one of claims 1 to 8.
10. Use of the protein fiber-immobilized zirconium-based activated carbon hybrid membrane according to claim 9 in removing sulfadiazine.
Citation Information
Cited By
Fiber hybrid membrane for synchronously removing radioactive cesium and strontium as well as preparation method and application of fiber hybrid membrane
CN120586685A
Nano flocculant as well as preparation method and application thereof
CN120864653A
Zirconium-based composite filler for removing antibiotics in wastewater based on artificial ecological wetland
CN121974495A