Method for improving tensile strength of mulberry silk

Through thermal stretching and amine functionalized graphene oxide technology, combined with cocoon boiling liquid of Ganoderma lucidum and wood ash, the tensile strength of mulberry silk is improved, the problem of poor durability of mulberry silk products is solved, and the preparation of high-performance silk is realized. It has sleep-aided effects in various application scenarios.

CN119083158AInactive Publication Date: 2024-12-06ZHEJIANG HUZHOU HAOSHENG SILK CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411388963.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The tensile strength of mulberry silk is poor, which makes the product not durable and difficult to meet the needs of various applications.

Method used

Through the combination technology of thermal stretching and amine-functionalized graphene oxide, the β-fold nanocrystal content and crystal orientation of silk are improved, and the cocoon liquid of Ganoderma lucidum and wood ash is degummed to form silk with high tensile strength.

Benefits of technology

It significantly improves the mechanical properties and durability of silk and is suitable for a variety of application scenarios, such as the preparation of high-performance medical materials and household products, and also has a sleep-aided effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083158A_ABST
    Figure CN119083158A_ABST
Patent Text Reader

Abstract

The invention relates to a method for improving the tensile strength of mulberry silk. The method comprises the steps of hot stretching of degummed silk, preparation of a silk-containing micro-nano fibrous protein solution, preparation of amine functionalized graphene oxide and preparation of high-tensile-strength silk. Wherein the preparation process of the degummed silk further comprises the steps of silkworm cocoon pretreatment, silkworm cocoon cooking liquid preparation, silkworm cocoon cooking and degumming and silk air drying. According to the mulberry silk improved through the technological process, the process is environmentally friendly, the tensile strength of the mulberry silk can reach 800 MPa, a pillow or a bed made of the mulberry silk can emit the fresh scent of sleep-aiding factors, the sleep-aiding effect is improved, and the mulberry silk has wide application prospects and market value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of silk, and in particular to a method for improving the tensile strength of mulberry silk. Background Art

[0002] Silk is a natural protein fiber. It was first used as a textile fiber to make clothing, quilts, etc. In recent years, with the in-depth study of silk, more application areas of silk have been explored. Silk is used as a biocompatible medical material due to its excellent mechanical properties, biocompatibility, and controllable biodegradability. It is used in tissue engineering, wound dressings, drug sustained release, medical sutures, and many other fields.

[0003] Moreover, as a natural fiber, the production process of mulberry silk has less impact on the environment. Compared with synthetic fibers, mulberry silk is more easily degraded in the natural environment and will not cause long-term environmental pollution. Therefore, choosing mulberry silk fabrics is not only an investment in personal health, but also a manifestation of environmental responsibility.

[0004] However, although mulberry silk is a high-quality and high-grade natural fiber, it also has some disadvantages. Mulberry silk products have poor elasticity and their tensile strength is not that good. People need to be careful when using them, and they are not very durable. Therefore, improving the tensile strength of mulberry silk raw materials has become an important issue. Summary of the invention

[0005] The technical purpose of the present invention is to solve the problems in the background technology and provide a method for improving the tensile strength of mulberry silk.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A method for improving the tensile strength of mulberry silk, the process of improving the tensile strength comprises the following steps: Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 150°C-200°C for a certain period of time, then stretching the silk fiber axially to a certain ratio, and keeping the temperature at 150°C-200°C for a certain period of time, and finally cooling the stretched silk to room temperature in argon to obtain hot stretched silk; Step S2: Preparation of a solution containing silk micro-nano fibrin protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 10-20 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fibrin protein; Step S3: Preparation of amine-functionalized graphene oxide: dispersing graphene in deionized water, adding p-phenylenediamine and isoamylamine nitrite and mixing evenly after dispersion, reacting the mixture at 60-100° C. for a certain period of time and then cooling to room temperature, and finally washing with acetone and deionized water for 2-4 times respectively and freeze-drying to obtain the amine-functionalized graphene oxide; Step S4: Preparation of high tensile strength silk: firstly, the amine-functionalized graphene oxide prepared in step S3 is dispersed in the solution prepared in step S2, and then the degummed silk fibers are added and immersed to form uniform spinning holes, and the high tensile strength silk is obtained by drying in a natural environment.

[0007] The advantage of adopting the present invention is that in step S1, a heat stretching process is first applied to the degummed silk, which can increase the content and crystal orientation of β-folded nanocrystals while retaining the components of the original silk fibers, thereby improving the mechanical properties and effectively and efficiently producing strong silk fibers.

[0008] Preferably, the degummed mulberry silk in step S1 is prepared by the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 10-20% water for later use; Step P2: preparing cocoon boiling liquid: taking two or more raw materials of Ganoderma lucidum, wild ginseng, Eucommia ulmoides, Scutellaria baicalensis, Crataegus pinnatifida, and Lysimachia chinensis and steaming them with water, filtering and obtaining a steaming solution for later use; Step P3: Steaming and degumming silkworm cocoons: Soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silkworm cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, then take the soaked silk and add it to the cocoon boiling liquid prepared in step P2, and steam and degumming them together under high temperature and high pressure; Step P4: air-drying the silk: putting the steamed silk into a windless drying environment for drying to obtain degummed silk.

[0009] Preferably, in the step P2, the cocoon cooking liquid is prepared by using Ganoderma lucidum, wild ginseng, Scutellaria baicalensis and hawthorn, wherein the mass fraction of Ganoderma lucidum is 5-10 parts, the mass fraction of wild ginseng, Scutellaria baicalensis and hawthorn is 1-5 parts respectively, and the rest is water; in the step P3, the mass volume fraction of plant ash in water is 10-20w / v%, and the number of cocoons to be cooked is not excessive, the mass ratio of cocoon cooking liquid to water in the cooking pot is 1:2, and the cocoons are cooked and degummed together under high temperature and high pressure, the temperature is controlled between 95-100°C, the cooking time is 45-60min, and the cocoons are stirred every 5min.

[0010] Preferably, in step P4, the windless drying temperature of the silk is controlled at 45°C.

[0011] The invention has the advantages that ganoderma lucidum is added to the cocoon boiling liquid and the silk is first soaked in plant ash water, the ganoderma lucidum water is combined with the plant ash alkaline water, the cocoons are boiled and degummed, which is not only very environmentally friendly, but also improves sleep and emits the fragrance of the noodle cooking factor.

[0012] The present invention has the advantage that the wild ginseng, rhizoma scutellariae and hawthorn used in the raw materials of the cocoon boiling liquid in step P2 are all very good Chinese herbal medicines; the liquid boiled with a unique ratio is combined with sericin and injected into the pores of the silk itself. Long-term use and contact with such silk products are beneficial to health.

[0013] Preferably, the degummed silk in step S1 is heated in argon at 180°C for 6 minutes, and then the silk fiber is stretched axially to a stretching rate of 2.5%-10%, and kept at 180°C for 6 minutes.

[0014] The advantage of adopting the present invention is that thermal stretching enhances the crystal orientation in the silk fiber. The improved crystallinity and enhanced crystal alignment make the thermally stretched silk fiber have excellent mechanical properties, which has a positive effect on the subsequent graphene functionalization.

[0015] Preferably, in the preparation of the silk micro-nano fibril protein solution in step S2, the mass concentration of the calcium chloride-formic acid solution is 4 w / v%.

[0016] Preferably, in the preparation of amine-functionalized graphene oxide in step S3, the graphene is functionalized by a diazo-hydrochloric acid method, and the parameters in the specific process are: the mass fraction of graphene is 1-3 parts, and the mass fractions of p-phenylenediamine and isoamylamine nitrite are 0.5-1 parts respectively.

[0017] Preferably, in step S3, the mixture is reacted at 80° C. for 10 h, cooled to room temperature, and washed three times with acetone and deionized water, respectively.

[0018] The present invention has the advantage of continuously producing ultra-strong and tough regenerated silk fibers (RSF) by reconstructing the layered and cross-linked structures. Amine-functionalized graphene (NH-G) is introduced to increase the β-folding content and crystal orientation, and glutaraldehyde (GA) is used to bridge NH-G and silk micro / nanofibrils (SNF) to form a highly interconnected and tightly packed network, resulting in significantly improved mechanical properties. The resulting fibers have excellent tensile strength and Young's modulus.

[0019] Preferably, in the preparation of high tensile strength silk in step S4, the mass fraction of the amine-functionalized graphene oxide in step S3 in the silk micro-nanofibril protein solution in step S2 is 0.2-0.8%.

[0020] Preferably, in the step S4, during the soaking process of the degummed silk fibers, each soaking time is 3-10 seconds, the number of soaking times is 25-40 times, and the interval between each soaking is 5-40 seconds.

[0021] The advantage of adopting the present invention is that through the specific immersion process of this scheme, the tensile properties brought to the silk by the graphene functionalization can be more thoroughly improved, so that when the silk prepared by this scheme is prepared into products such as pillows or bedding, it can not only play its unique sleep-inducing and calming effect, but also improve its durability and tensile resistance, and is less likely to break.

[0022] In summary, the present invention has the following beneficial effects: 1. By combining Ganoderma lucidum with plant ash alkaline water, it can better play the role of helping sleep, emit the fragrance of cooking factors, and provide a guarantee for users to have a good rest and sleep; 2. The degumming of silkworm cocoons and silk uses the best Chinese herbal medicine, which is very environmentally friendly and harmless to the environment, responding to the current call for green health and environmental protection; 3. Through the hot stretching process in step S1, the content and crystal orientation of β-folded nanocrystals can be increased while retaining the composition of the original silk fiber, thereby improving the mechanical properties and effectively and efficiently producing strong silk fibers; 4. By subjecting the degummed silk cocoons / silk to graphene functionalization conditions specially customized for this solution, the obtained silk products have excellent tensile strength and Young's modulus, and can be used to prepare high-performance silk fibers with broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] FIG. 1 is a process flow chart of a method for improving the tensile strength of mulberry silk. DETAILED DESCRIPTION

[0024] The following specific embodiments are merely explanations of the present invention and are not limitations of the present invention. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, such modifications are protected by the patent law as long as they are within the scope of the claims of the present invention.

[0025] Example 1

[0026] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 2.5%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fiber protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 10 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fiber protein; Step S3: Preparation of amine-functionalized graphene oxide: 1 part of graphene is dispersed in deionized water, and after the dispersion is completed, 0.5 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.2%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 3 seconds, the number of soaking times is 40 times, and the interval between each soaking is 5 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0027] The degummed silk in step S1 is obtained by processing the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 10% water for later use; Step P2: preparing the cocoon cooking liquid: the cocoon cooking liquid is prepared by using Ganoderma lucidum, wild ginseng, Scutellaria baicalensis and hawthorn, wherein the mass fractions of Ganoderma lucidum are 5 parts, the mass fractions of wild ginseng, Scutellaria baicalensis and hawthorn are 5 parts respectively, and the rest is water; filtering to obtain the cooking solution, which is set aside; Step P3: Steaming and degumming silk cocoons: soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silk cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, the mass volume fraction of wood ash in water is 10w / v%, and the number of steamed silk cocoons is not excessive, the mass ratio of the cocoon boiling liquid to the added water in the steaming pot is 1:2, and steam and degumming are carried out together under high temperature and high pressure, the temperature is controlled between 95-100°C, the steaming time is 45min, and stirring is performed every 5min; Step P4: air-drying the silk: placing the steamed silk in a windless drying environment for drying, with the drying temperature controlled at 45°C, to obtain degummed silk.

[0028] Example 2

[0029] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 10%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fiber protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 20 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fiber protein; Step S3: Preparation of amine-functionalized graphene oxide: 3 parts of graphene are dispersed in deionized water, and after the dispersion is completed, 1 part of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.8%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 10 seconds, the number of soaking times is 25 times, and the interval between each soaking is 40 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0030] The degummed silk in step S1 is obtained by processing the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 20% water for later use; Step P2: preparing the cocoon cooking liquid: the cocoon cooking liquid is prepared by using Ganoderma lucidum, wild ginseng, Scutellaria baicalensis and hawthorn, wherein the mass fraction of Ganoderma lucidum is 10 parts, the mass fraction of wild ginseng, Scutellaria baicalensis and hawthorn is 1 part respectively, and the rest is water; filtering to obtain the cooking solution, which is set aside; Step P3: Steaming and degumming silk cocoons: soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silk cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, the mass volume fraction of wood ash in water is 20w / v%, and the number of steamed silk cocoons is not excessive, the mass ratio of the cocoon boiling liquid to the added water in the steaming pot is 1:2, and steam and degumming are carried out together under high temperature and high pressure, the temperature is controlled between 95-100°C, the steaming time is 60min, and stirring is performed every 5min; Step P4: air-drying the silk: placing the steamed silk in a windless drying environment for drying, with the drying temperature controlled at 45°C, to obtain degummed silk.

[0031] Example 3

[0032] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 5%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fibril protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 18 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fibril protein; Step S3: Preparation of amine-functionalized graphene oxide: 1-3 parts of graphene are dispersed in deionized water, and after the dispersion is completed, 0.8 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, and the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.3%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 8 seconds, the number of soaking times is 28 times, and the interval between each soaking is 30 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0033] The degummed silk in step S1 is obtained by processing the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 12% water for later use; Step P2: preparing the cocoon cooking liquid: the cocoon cooking liquid is prepared by using ganoderma lucidum, wild ginseng, scutellaria baicalensis and hawthorn, wherein the mass fractions of ganoderma lucidum are 9 parts, the mass fractions of wild ginseng, scutellaria baicalensis and hawthorn are 3 parts respectively, and the rest is water; filtering to obtain the cooking solution, which is set aside; Step P3: Steaming and degumming silk cocoons: soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silk cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, the mass volume fraction of wood ash in water is 14w / v%, and the number of steamed silk cocoons is not excessive, the mass ratio of the cocoon boiling liquid to the added water in the steaming pot is 1:2, and steam and degumming are carried out together under high temperature and high pressure, the temperature is controlled between 95-100°C, the steaming time is 50min, and stirring is performed every 5min; Step P4: air-drying the silk: placing the steamed silk in a windless drying environment for drying, with the drying temperature controlled at 45°C, to obtain degummed silk.

[0034] Example 4

[0035] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 7.5%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fiber protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 15 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fiber protein; Step S3: Preparation of amine-functionalized graphene oxide: 2.7 parts of graphene are dispersed in deionized water, and after the dispersion is completed, 0.9 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, and the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.5%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 8 seconds, the number of soaking times is 33 times, and the interval between each soaking is 32 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0036] The degummed silk in step S1 is obtained by processing the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 15% water for later use; Step P2: preparing the cocoon cooking liquid: the cocoon cooking liquid is prepared by using Ganoderma lucidum, wild ginseng, Scutellaria baicalensis and hawthorn, wherein the mass fractions of Ganoderma lucidum are 8 parts, the mass fractions of wild ginseng, Scutellaria baicalensis and hawthorn are 2.5 parts respectively, and the rest is water; filtering to obtain the cooking solution, which is set aside; Step P3: Steaming and degumming silk cocoons: soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silk cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, the mass volume fraction of wood ash in water is 16w / v%, and the number of steamed silk cocoons is not excessive, the mass ratio of the cocoon boiling liquid to the added water in the steaming pot is 1:2, and steam and degumming are carried out together under high temperature and high pressure, the temperature is controlled between 95-100°C, the steaming time is 55min, and stirring is performed every 5min; Step P4: air-drying the silk: placing the steamed silk in a windless drying environment for drying, with the drying temperature controlled at 45°C, to obtain degummed silk.

[0037] Example 5

[0038] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 7.5%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fiber protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 15 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fiber protein; Step S3: Preparation of amine-functionalized graphene oxide: 2.5 parts of graphene are dispersed in deionized water, and after the dispersion is completed, 0.85 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, and the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.5%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 8 seconds, the number of soaking times is 30 times, and the interval between each soaking is 30 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0039] The degummed silk in step S1 is obtained by processing the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 15% water for later use; Step P2: preparing the cocoon cooking liquid: the cocoon cooking liquid is prepared by using Ganoderma lucidum, wild ginseng, Scutellaria baicalensis and hawthorn, wherein the mass fractions of Ganoderma lucidum are 5 parts, the mass fractions of wild ginseng, Scutellaria baicalensis and hawthorn are 1 part respectively, and the rest is water; filtering to obtain the cooking solution, which is set aside; Step P3: Steaming and degumming silk cocoons: soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silk cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, the mass volume fraction of wood ash in water is 18w / v%, and the number of steamed silk cocoons is not excessive, the mass ratio of the cocoon boiling liquid to the added water in the steaming pot is 1:2, and steam and degumming are carried out together under high temperature and high pressure, the temperature is controlled between 95-100°C, the steaming time is 45min, and stirring is performed every 5min; Step P4: air-drying the silk: placing the steamed silk in a windless drying environment for drying, with the drying temperature controlled at 45°C, to obtain degummed silk.

[0040] Example 6

[0041] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 7.5%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fiber protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 15 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fiber protein; Step S3: Preparation of amine-functionalized graphene oxide: 2.5 parts of graphene are dispersed in deionized water, and after the dispersion is completed, 0.85 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, and the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.5%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 8 seconds, the number of soaking times is 30 times, and the interval between each soaking is 30 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0042] The degummed silk in step S1 is obtained by processing the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 20% water for later use; Step P2: preparing the cocoon cooking liquid: the cocoon cooking liquid is prepared by using Ganoderma lucidum, wild ginseng, Scutellaria baicalensis and hawthorn, wherein the mass fractions of Ganoderma lucidum are 9 parts, the mass fractions of wild ginseng, Scutellaria baicalensis and hawthorn are 3.3 parts respectively, and the rest is water; filtering to obtain the cooking solution, which is set aside; Step P3: Steaming and degumming silk cocoons: soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silk cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, the mass volume fraction of wood ash in water is 20w / v%, and the number of steamed silk cocoons is not excessive, the mass ratio of the cocoon boiling liquid to the added water in the steaming pot is 1:2, and steam and degumming are carried out together under high temperature and high pressure, the temperature is controlled between 95-100°C, the steaming time is 48min, and stirring is performed every 5min; Step P4: air-drying the silk: placing the steamed silk in a windless drying environment for drying, with the drying temperature controlled at 45°C, to obtain degummed silk.

[0043] Comparative Example 1

[0044] Different from the above-mentioned embodiment, this comparative example does not adopt the same silkworm boiling and degumming step as the above-mentioned embodiment, but adopts the more common chemical degumming method for treating silk.

[0045] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180° C. for 6 minutes, then stretching the silk fiber axially to a stretching rate of 7.5%, and keeping the temperature at 180° C. for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain silk after the hot stretching process; Step S2: Preparation of a solution containing silk micro-nano fiber protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 15 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fiber protein; Step S3: Preparation of amine-functionalized graphene oxide: 2.5 parts of graphene are dispersed in deionized water, and after the dispersion is completed, 0.85 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, and the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S4 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S3 in the solution prepared in the step S2, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.5%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 8 seconds, the number of soaking times is 30 times, and the interval between each soaking is 30 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0046] The degummed silk in the above step S1 is subjected to chemical degumming treatment, i.e., alkaline reagent, acidic reagent, surfactant, protease and high temperature and high pressure treatment.

[0047] Comparative Example 2

[0048] Different from the comparative example 1 mentioned above, the pre-treatment of the silk in this comparative example adopts chemical degumming, and the heat stretching process in step S1 of the invention scheme is omitted.

[0049] Step S1: Preparation of a silk-containing micro-nano fiber protein solution: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a 4 w / v% calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 15 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a silk-containing micro-nano fiber protein solution; Step S2: Preparation of amine-functionalized graphene oxide: 2.5 parts of graphene are dispersed in deionized water, and after dispersion, 0.85 parts of p-phenylenediamine and isoamylamine nitrite are added respectively and mixed evenly, the mixture is reacted at 80° C. for 10 hours and then cooled to room temperature, washed with acetone and deionized water for 3 times respectively, and freeze-dried to obtain the amine-functionalized graphene oxide; Step S3 preparation of high tensile strength silk: first disperse the amine-functionalized graphene oxide prepared in the step S2 in the solution prepared in the step S1, the mass fraction of the amine-functionalized graphene oxide in the step S2 in the silk micro-nanofibril protein solution in the step S1 is 0.5%, and then add the degummed silk fibers to soak to form uniform spinning holes. During the soaking process, each soaking time is 8 seconds, the number of soaking times is 30 times, and the interval between each soaking is 30 seconds; finally, dry in a natural environment to obtain the high tensile strength silk.

[0050] Comparative Example 3

[0051] Different from the above-mentioned comparative example 2, this comparative example adopts chemical degumming to treat silk, retains the heat stretching step, but does not have the subsequent graphene functionalization step.

[0052] Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 180°C for 6 minutes, then stretching the silk fiber axially to a stretching rate of 7.5%, and keeping it at 180°C for 6 minutes, and finally cooling the stretched silk to room temperature in argon to obtain the silk after the hot stretching process.

[0053] Comparative Example 4

[0054] This comparative example is the silk that has only been treated with chemical degumming.

[0055] The tensile strength of the mulberry silk products tested in the above Examples 1-6 and Comparative Examples 1-4 is shown in Table 1 below: Table 1 Data results of Examples 1-6

[0056] The data results of Comparative Examples 1-4 are shown in Table 2 below: Table 2 Comparative Examples 1-4 Data Results Table

[0057] It can be seen from the above table data that in Examples 1-6, the highest tensile strength can be obtained by preparing silk using the process parameters in Example 4, and the tensile strength reaches 856.3 MPa.

[0058] Compared with Examples 1 and 2, since the minimum or maximum endpoint values ​​of the process parameters are limited during the preparation process, the tensile strength of the prepared silk can only reach about 725 MPa.

[0059] Compared with Example 3, the stretching process and functionalization process parameters of Step S1 to Step S4 were adjusted significantly, and the obtained silk tensile strength was slightly better than that of Examples 1 and 2, but also lower than that of Example 4, reaching 742.1 MPa.

[0060] Compared with Examples 5 and 6, Examples 5 and 6 have greatly adjusted the process parameters of steps P1-P4, but the impact brought about is not as great as that of steps S1-S4. Therefore, it can be preliminarily determined that the stretching and amine functionalized graphene process of steps S1-S4 has a more decisive effect on the tensile strength of silk.

[0061] In Comparative Example 1, the degumming method of silk cocoons adopts the currently common chemical degumming method, but it is still subjected to thermal stretching and graphene functionalization process subsequently, and its tensile strength is also acceptable, reaching 704MPa.

[0062] In Comparative Examples 2 and 3, chemical degumming is used. The former abandons the thermal stretching process, and the latter abandons the graphene functionalization process. It can be seen that the tensile properties of the silk finally obtained are poor, only around 410MPa.

[0063] Comparative Example 4 did not undergo any of the same processes as in this solution, so its tensile strength was the lowest, only 359.8 MPa, which further illustrates that the process added in this solution plays an important role in improving the tensile strength of silk.

Claims

1. A method for improving the tensile strength of mulberry silk, characterized in that: The process of improving tensile strength comprises the following steps: Step S1: hot stretching of degummed silk: using degummed silk as raw material, heating the degummed silk in argon at 150°C-200°C for a certain period of time, then stretching the silk fiber axially to a certain ratio, and keeping the temperature at 150°C-200°C for a certain period of time, and finally cooling the stretched silk to room temperature in argon to obtain hot stretched silk; Step S2: Preparation of a solution containing silk micro-nano fibrin protein: Slice and wash the degummed silk cocoons, dissolve the washed degummed silk in a calcium chloride-formic acid solution, wherein the mass fraction of the degummed silk in the solution is 10-20 parts, and the rest is the calcium chloride-formic acid solution; after the solution is evenly dissolved and dispersed, remove the excess formic acid to obtain a solution containing silk micro-nano fibrin protein; Step S3: Preparation of amine-functionalized graphene oxide: dispersing graphene in deionized water, adding p-phenylenediamine and isoamylamine nitrite and mixing evenly after dispersion, reacting the mixture at 60-100° C. for a certain period of time and then cooling to room temperature, and finally washing with acetone and deionized water for 2-4 times respectively and freeze-drying to obtain the amine-functionalized graphene oxide; Step S4: Preparation of high tensile strength silk: firstly, the amine-functionalized graphene oxide prepared in step S3 is dispersed in the solution prepared in step S2, and then the degummed silk fibers are added and immersed to form uniform spinning holes, and the high tensile strength silk is obtained by drying in a natural environment.

2. A method for improving the tensile strength of mulberry silk according to claim 1, characterized in that: The degummed mulberry silk in step S1 is prepared by the following steps: Step P1: pre-treatment of silk cocoons: clean the silk cocoons or silk and immerse them in water to make the water content of the silk cocoons or silk into 10-20% water for later use; Step P2: preparing cocoon boiling liquid: taking two or more raw materials of Ganoderma lucidum, wild ginseng, Eucommia ulmoides, Scutellaria baicalensis, Crataegus pinnatifida, and Lysimachia chinensis and steaming them with water, filtering and obtaining a steaming solution for later use; Step P3: Steaming and degumming silkworm cocoons: Soak an appropriate amount of wood ash in water for 3 hours, take the concentrated juice after precipitation and filter it into a porcelain jar, then put an appropriate amount of silkworm cocoons from step P1 into the porcelain jar and soak them in warm water for 12 hours, then take the soaked silk and add it to the cocoon boiling liquid prepared in step P2, and steam and degumming them together under high temperature and high pressure; Step P4: air-drying the silk: putting the steamed silk into a windless drying environment for drying to obtain degummed silk.

3. A method for improving the tensile strength of mulberry silk according to claim 2, characterized in that: In the step P2, the cocoon-cooking liquid is prepared by using ganoderma lucidum, wild ginseng, scutellaria baicalensis and hawthorn, wherein the mass fraction of ganoderma lucidum is 5-10 parts, the mass fraction of wild ginseng, scutellaria baicalensis and hawthorn is 1-5 parts respectively, and the rest is water; in the step P3, the mass volume fraction of plant ash in water is 10-20w / v%, and the number of cocoons to be cooked is not excessive, the mass ratio of cocoon-cooking liquid to water in the cooking pot is 1:2, and the cocoons are cooked and degummed together under high temperature and high pressure, the temperature is controlled between 95-100°C, the cooking time is 45-60min, and the silk is stirred every 5min; in the step P4, the windless drying temperature of the silk is controlled at 45°C.

4. The method for improving the tensile strength of mulberry silk according to claim 1, characterized in that: In the step S1, the degummed silk is heated in argon at 180° C. for 6 minutes, and then the silk fiber is stretched axially to a stretching rate of 2.5%-10%, and then kept at 180° C. for 6 minutes.

5. The method for improving the tensile strength of mulberry silk according to claim 1, characterized in that: In the preparation of the silk micro-nano fibrin solution in step S2, the mass concentration of the calcium chloride-formic acid solution is 4 w / v%.

6. The method for improving the tensile strength of mulberry silk according to claim 1, characterized in that: In the preparation of amine-functionalized graphene oxide in step S3, the graphene is functionalized by a diazo-hydrochloric acid method, and the parameters in the specific process are: the mass fraction of graphene is 1-3 parts, and the mass fractions of p-phenylenediamine and isoamylamine nitrite are 0.5-1 parts respectively.

7. A method for improving the tensile strength of mulberry silk according to claim 6, characterized in that: In step S3, the mixture is reacted at 80° C. for 10 h, cooled to room temperature, and washed three times with acetone and deionized water respectively.

8. The method for improving the tensile strength of mulberry silk according to claim 1, characterized in that: In the step S4 of preparing high tensile strength silk, the mass fraction of the amine-functionalized graphene oxide in the step S3 in the silk micro-nanofibril protein solution in the step S2 is 0.2-0.8%.

9. The method for improving the tensile strength of mulberry silk according to claim 1, characterized in that: In the step S4, during the soaking process of the degummed silk fibers, each soaking time is 3-10 seconds, the number of soaking times is 25-40 times, and the interval between each soaking is 5-40 seconds.

10. A mulberry silk, characterized in that: The mulberry silk is prepared by the method for high tensile strength of mulberry silk according to any one of claims 1 to 9. The prepared mulberry silk has high tensile strength and a sleep-aiding effect, and has a prolonged service life, and can be applied to the fields of silk pillows, beds, etc.