Ag-coated beta-cyclodextrin fiber-based SERS (Surface Enhanced Raman Scattering) substrate as well as preparation method and application thereof in printing and dyeing wastewater detection
By constructing a flower-like Ag@β-cyclodextrin fiber-based SERS substrate on fiber materials, combining electromagnetic field and chemical enhancement, the problem of insufficient detection sensitivity in textile printing and dyeing wastewater is solved, high sensitivity detection of methylene blue is achieved, and wastewater is promoted Applications for processing and reuse.
Patent Information
- Application Number
- CN202411183808.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art has insufficient detection sensitivity in textile printing and dyeing wastewater, making it difficult to effectively detect pollutants such as methylene blue, resulting in water pollution problems.
A Ag@β-cyclodextrin fiber-based SERS substrate was developed, which was prepared by attaching modified silver nanoparticles to the fiber material in a flower-like structure, using ascorbic acid reduction method, combining electromagnetic field and chemical enhancement effects to improve Raman signal .
The minimum detection concentration of methylene blue is achieved to reach 1.0×10-10mol L-1, which significantly improves the detection sensitivity and provides a fast and accurate detection solution.
Smart Images

Figure CN119083162A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of detection, and in particular to an Ag@β-cyclodextrin fiber-based SERS substrate, a preparation method thereof, and application thereof in the detection of printing and dyeing wastewater. Background Art
[0002] There are many types of dyes, which are widely used in many industries such as food, fiber, leather, papermaking, etc., especially in the textile and printing and dyeing industry. In the refining process of textiles, a large amount of water, mineral salts and reactive dyes are needed. Therefore, a large amount of dye wastewater will be generated, which contains many pollutants. Textile printing and dyeing wastewater usually contains various types of dyes, detergents and solvents, depending on the specific process of textile and printing and dyeing, such as scouring, bleaching, dyeing, printing, finishing, etc. Dye wastewater is dark in color, has a large pH value fluctuation, and contains suspended solids, organic matter, metals and salts. Typical textile wastewater is difficult to define because even in the same process, the use of textile wastewater varies from industry to industry. So far, methylene blue has been widely used in the textile printing and dyeing industry, bringing great convenience to people's production and life. However, in order to save costs and obtain greater economic benefits, some unscrupulous businesses fail to properly treat textile printing and dyeing wastewater, causing some residual methylene blue to flow into the water environment and continue to accumulate, causing certain water pollution and endangering human health. Therefore, effective detection of pollutants in wastewater has great application prospects in the treatment, recycling and reuse of textile printing and dyeing wastewater in the future.
[0003] Raman scattering is an inelastic scattering phenomenon. Currently, Raman scattering is widely used in chemistry, biology, materials science and other fields. For example, by analyzing Raman scattering spectra, we can understand the chemical bonds and structures of molecules; Raman spectroscopy can be used to study the chemical composition of cells and tissues; Raman spectroscopy can be used to characterize the crystal structure and defects of materials. Therefore, Raman scattering is a very useful analytical tool. However, due to the fact that the Raman scattering signal is usually weak, the sensitivity of using Raman scattering to detect printing and dyeing wastewater is currently insufficient.
[0004] Surface-enhanced Raman scattering (SERS) technology is a method that uses electromagnetic field and chemical signal enhancement based on Raman scattering. SERS has quickly become a popular detection method in the field of chemical analysis due to its high sensitivity, non-destructiveness to samples, high selectivity, and fast data analysis.
[0005] Therefore, it is of great significance to develop a new Ag@β-cyclodextrin fiber-based SERS substrate and explore its application in printing and dyeing wastewater. Summary of the invention
[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide an Ag@β-cyclodextrin SERS substrate with a flower-like structure, a high specific surface area and a SERS enhancement effect in view of the deficiencies in the prior art.
[0007] In order to solve the above technical problems, the present invention discloses an Ag@β-cyclodextrin fiber-based SERS substrate, which is constructed by attaching β-cyclodextrin-modified silver nanoparticles to the surface of a fiber material; wherein the silver nanoparticles have a flower-like structure.
[0008] Wherein, the Ag@β-cyclodextrin fiber-based SERS substrate is prepared by ascorbic acid reduction method; and the Ag source in the Ag@β-cyclodextrin fiber-based SERS substrate is silver nitrate.
[0009] The present invention also provides a method for preparing an Ag@β-cyclodextrin fiber-based SERS substrate, the specific steps of which include:
[0010] S1. Cut and clean fiber materials;
[0011] S2. Prepare a β-cyclodextrin solution, and add the fiber material washed in step S1 into the β-cyclodextrin solution to fully immerse it;
[0012] S3. Prepare a silver nitrate solution and add it to the β-cyclodextrin solution containing the fiber material in step S2, and stir to obtain a mixture solution;
[0013] S4. Prepare an ascorbic acid solution and add it to the mixture solution of step S3, and obtain the Ag@β-cyclodextrin fiber-based SERS substrate after stirring and centrifugal drying.
[0014] Preferably, in step S2, the concentration of the β-cyclodextrin solution is 0.8 to 1.2 mmol L -1 ;
[0015] More preferably, in step S2, the concentration of the β-cyclodextrin solution is 1 mmol L -1 ;
[0016] Preferably, in step S3, the concentration of the silver nitrate solution is 0.08 to 0.12 mmol L -1 ;
[0017] More preferably, in step S3, the concentration of the silver nitrate solution is 0.1 mmol L -1 ;
[0018] Preferably, in step S4, the concentration of the ascorbic acid solution is 0.08 to 0.12 mmol L -1 ;
[0019] More preferably, in step S4, the concentration of the ascorbic acid solution is 0.1 mmol L -1 ;
[0020] Preferably, the volume ratio of the β-cyclodextrin solution, the silver nitrate solution and the ascorbic acid solution is (8-12):1:1;
[0021] More preferably, the volume ratio of the β-cyclodextrin solution, the silver nitrate solution and the ascorbic acid solution is 10:1:1;
[0022] Preferably, in step S4, the rotation speed during centrifugation is 6000-10000 rpm;
[0023] More preferably, in step S4, the rotation speed during centrifugation is 8000 rpm.
[0024] The application of the above-mentioned Ag@β-cyclodextrin fiber-based SERS substrate in the detection of printing and dyeing wastewater is also within the scope of protection of the present invention.
[0025] Wherein, the printing and dyeing wastewater includes but is not limited to methylene blue.
[0026] The detection concentration range of the Ag@β-cyclodextrin fiber-based SERS substrate in printing and dyeing wastewater is 1.0×10 -10 ~1.0×10 -4 mol L -1 .
[0027] Beneficial effects: The present invention prepares a flower-shaped Ag@β-CD SERS substrate, which has obvious Raman signal enhancement for methylene blue. This is attributed to the fact that the SERS substrate prepared by the present invention has both electromagnetic field enhancement and chemical enhancement. The electromagnetic enhancement of the flower-shaped Ag@β-CD as a SERS substrate comes from the methylene blue being in the localized plasma resonance region of the Ag particles. The chemical enhancement comes from β-CD, when the methylene blue enters the β-CD cavity and directly contacts the Ag particles, producing chemical enhancement.
[0028] The Ag@β-CD SERS substrate prepared by the present invention can be used to detect methylene blue. Through in-depth analysis of the interaction between the SERS substrate and the methylene blue molecules, the Ag@β-CD SERS substrate prepared by the present invention can detect the minimum concentration of methylene blue up to 1.0×10 -10 mol L -1 .
[0029] The present invention constructs an Ag@β-CD fiber-based SERS substrate and explores its application in the detection of textile printing and dyeing wastewater. Through experimental analysis and data verification, the detection performance and stability of the substrate are studied to provide a better solution for the rapid detection of chemical dyes such as methylene blue. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0031] Figure 1 Schematic diagram of the preparation of flower-shaped Ag@β-CD in an embodiment of the present invention;
[0032] Figure 2 This is a SEM image of the flower-shaped Ag@β-CD in the embodiment of the present invention;
[0033] Figure 3 This is the XRD analysis diagram of the flower-shaped Ag@β-CD in the embodiment of the present invention;
[0034] Figure 4 This is a Fourier transform infrared spectrum test diagram of the flower-shaped Ag@β-CD in the embodiment of the present invention;
[0035] Figure 5 Schematic diagram of the preparation of Ag@β-CD fiber-based SERS substrate in an embodiment of the present invention;
[0036] Figure 6 This is a SEM image of the Ag@β-CD fiber-based SERS substrate in an embodiment of the present invention;
[0037] Figure 7 The standard absorbance curve of methylene blue in the embodiment of the present invention;
[0038] Figure 8 This is a graph showing the adsorption amount of flower-shaped Ag@β-CD for methylene blue solution of the same concentration at different adsorption times in an embodiment of the present invention;
[0039] Fig. 9 This is a graph showing the adsorption of methylene blue solutions of different concentrations by flower-shaped Ag@β-CD after oscillation for 1 hour in the embodiment of the present invention;
[0040] Fig.10 This is a graph showing the adsorption of methylene blue solutions of different concentrations by flower-shaped Ag@β-CD after 2 hours of oscillation in the embodiment of the present invention;
[0041] Fig.11 This is a Raman detection image of methylene blue in an embodiment of the present invention;
[0042] Fig.12The Raman enhanced spectra of the flower-shaped Ag@β-CD SERS substrate to different concentrations of methylene blue in the embodiment of the present invention;
[0043] Fig.13 The following are pictures of the Ag@β-CD fiber-based SERS substrate after the addition of methylene blue solutions of different concentrations in the embodiments of the present invention;
[0044] Fig.14 This is the Raman enhanced spectrum of methylene blue of the Ag@β-CD fiber-based SERS substrate in the embodiment of the present invention. DETAILED DESCRIPTION
[0045] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0046] Example 1: Preparation of flower-shaped Ag@β-CD
[0047] Figure 1 Schematic diagram of the preparation of flower-like Ag@β-CD. 0.0565 g of β-CD was dissolved in 50 mL of deionized water. After complete dissolution, 5.0 mL (0.1 mmol L) of β-CD was added. -1 ) of silver nitrate aqueous solution. Stir at room temperature for 2 h. Add 5 mL (0.1 mmol L -1 ) of ascorbic acid, stirred at room temperature for 2 h to obtain a reaction mixture. The reaction mixture was centrifuged (8000 rpm) and washed with water for 3 times to obtain flower-like Ag@β-CD.
[0048] Example 2: Characterization and analysis of flower-like Ag@β-CD
[0049] The flower-like Ag@β-CD obtained in Example 1 was characterized by a field emission scanning electron microscope (Nova Nano SEM 450; FEI Company, USA), an X-ray diffractometer (XPERT3POWDER; PANalytical Company) and a Fourier transform infrared spectrometer (NEXUF-670; NICOLET, USA). The characterization results are as follows: Figures 2 to 4 shown.
[0050] Figure 2 This is the SEM image of the flower-shaped Ag@β-CD obtained in Example 1. It can be seen from the figure that the product prepared in Example 1 presents an irregular flower shape, which proves that the preparation method in Example 1 can prepare flower-shaped Ag@β-CD.
[0051] Figure 3This is the XRD analysis diagram of the flower-shaped Ag@β-CD obtained in Example 1. It can be seen from the figure that the characteristic diffraction peak positions of the (111), (200), (220), (311) and (222) crystal planes appear at 2θ=38.24°, 44.57°, 64.78°, 77.68° and 81.83°, respectively. Among them, the (111) crystal plane is the dominant crystal plane, which is due to its unique characteristics in the silver crystal structure. First, the (111) crystal plane is the most densely arranged crystal plane in the face-centered cubic (FCC) structure, with a close arrangement of atoms and the lowest energy, which makes it relatively stable during the formation process. Therefore, in the XRD diagram, the (111) diffraction peak of the flower-shaped silver is usually the strongest, indicating that it is the dominant crystal plane. The positions of these peaks match the positions of the XRD characteristic peaks of Ag, which also shows that the XRD spectrum of the prepared flower-shaped Ag@β-CD is consistent with the characteristic diffraction peaks of Ag in the face-centered cubic structure.
[0052] Figure 4 The Fourier transform infrared spectrum test results of the flower-shaped Ag@β-CD obtained in Example 1 are shown in the figure. As can be seen from the figure, the flower-shaped Ag@β-CD has a peak at 1626 cm -1 、2853cm -1 、2924cm -1 and 3441cm -1 Obvious infrared characteristic peaks appeared at 3441cm -1 The absorption peak at 1626 cm is attributed to the stretching vibration of the hydrophilic group -OH on the surface of β-CD. -1 The peak at is attributed to the stretching vibration of the C=C bond, from which it can be judged that β-CD is successfully coated on the Ag surface.
[0053] Example 3: Preparation of Ag@β-CD fiber-based SERS substrate
[0054] Figure 5 The schematic diagram of the preparation of Ag@β-CD fiber-based SERS substrate is shown in Figure 1. Cut a 2 cm × 1 cm fiber base and wash it for later use. Take 0.0565 g of β-CD and dissolve it in 50 mL of deionized water. After it is completely dissolved, add the washed fiber base to the β-CD solution. After the fiber base fully absorbs the solution, add 5.0 mL (0.1 mmol L -1 ) of silver nitrate aqueous solution, stirred at room temperature for 2 h, and then 5 mL (0.1 mmol L -1 ) of ascorbic acid, stirred at room temperature for 2 h to obtain a reaction mixture. The reaction mixture was centrifuged (8000 rpm), the fiber base was taken out, washed repeatedly with water for 3 times and dried to obtain a flower-like structured Ag@β-CD fiber-based SERS substrate.
[0055] Example 4: Characterization and analysis of Ag@β-CD fiber-based SERS substrate
[0056] The flower-like Ag@β-CD fiber matrix prepared in Example 3 was characterized by SEM. Figure 6 As shown in the figure, it can be seen that the flower-shaped Ag@β-CD is successfully attached to the fiber substrate and evenly loaded on the surface of the fiber substrate. It has the characteristics of flatness and density, making the subsequent Raman detection results of methylene blue more accurate. This also shows that the flower-shaped Ag@β-CD fiber-based SERS substrate has been successfully prepared.
[0057] Example 5: Verification of the adsorption capacity of Ag@β-CD on dyes in printing and dyeing wastewater
[0058] 1. Measure the standard absorbance curve of methylene blue dye; take 7 identical centrifuge tubes and add a certain amount of 1.0×10 -4 mol L -1 The methylene blue stock solution was then diluted to 1.0 × 10 -6 mol L -1 , 2.0×10 -6 mol L -1 , 5.0×10 -6 mol L -1 , 1.0×10 -7 mol L -1 , 2.0×10 -7 mol L -1 , 5.0×10 -7 mol L -1 , 5.0×10 -8 mol L -1 The absorbance of methylene blue solutions of various concentrations was measured using a double-beam UV-visible spectrophotometer (TU-1901; Beijing Puxi General Instrument Co., Ltd.), and then the standard absorbance curves of methylene blue solutions of different concentrations were plotted.
[0059] Figure 7 is the standard absorbance curve of methylene blue, from which we can get the relationship between absorbance and methylene blue solution concentration 1:
[0060] Y=199126.28X-0.0049;R 2 =0.9990 (1)
[0061] Where Y is the absorbance, X is the concentration of methylene blue solution; R 2 The value represents the correlation coefficient, which is used to express the correlation between the horizontal and vertical coordinates. Therefore, the formula can accurately reflect the relationship between absorbance and concentration.
[0062] After calculating the concentration of the methylene blue solution by absorbance, the adsorption amount of methylene blue by the flower-shaped Ag@β-CD was calculated based on the relationship between substrate concentration and adsorption amount. Equation 2 is:
[0063]
[0064] Where Q is the adsorption amount of methylene blue by flower-like Ag@β-CD; C0 is the initial concentration of the substrate before adsorption (mmol / L); Ceq is the concentration of the substrate at adsorption equilibrium (mmol / L); V is the volume of the solution (mL); and W is the mass of the solution (g).
[0065] Detecting the standard adsorption curve of methylene blue plays an important role in experiments and applications. First, by establishing a standard adsorption curve, the concentration of methylene blue in different samples can be accurately determined, thereby ensuring the reliability of the experimental results. Secondly, through the standard absorbance curve of methylene blue, the relationship between the absorbance and concentration of methylene blue can be obtained, which is convenient for observing the changing relationship between time and adsorption amount, and between concentration and adsorption amount in the form of a chart.
[0066] 2. Detection of the adsorption capacity of flower-shaped Ag@β-CD on methylene blue solution of the same concentration at different adsorption times; Study the adsorption capacity of flower-shaped Ag@β-CD on methylene blue dye after different adsorption times. Take 7 identical centrifuge tubes and add 8 mL of 1.0×10 -6 mol L -1 Methylene blue solution, add 20mg flower-shaped Ag@β-CD at the same time, and place it on an oscillator after ultrasonic treatment for one minute. Samples are taken at regular intervals, and the intervals are 0min, 1min, 5min, 10min, 30min, 1h, and 2h. The absorbance of methylene blue dye after different adsorption times is measured with a photometer, and then the adsorption amount of methylene blue dye by flower-shaped Ag@β-CD at the same concentration and different time is calculated using formula 1 and formula 2, and the corresponding time and adsorption amount graph is drawn.
[0067] Figure 8 This is the adsorption amount of Ag@β-CD for methylene blue solution of the same concentration at different adsorption times. It can be seen from the figure that the adsorption amount of methylene blue increases rapidly from 0 min to 60 min, and the adsorption growth rate gradually tends to be constant from 60 min to 120 min. It can be judged that it is most appropriate to control the adsorption time at 60 min, which can reduce the time and cost of experimental operation.
[0068] 3. Detection of the adsorption capacity of flower-shaped Ag@β-CD on methylene blue solutions of different concentrations and the same adsorption time; Study the adsorption capacity of flower-shaped Ag@β-CD on methylene blue dyes of different concentrations at the same adsorption time. Take 7 identical small centrifuge tubes, add 2 mL of methylene blue solution to each, and dilute it to 1.0×10 -6 mol L -1 , 2.0×10 -6 mol L -1 , 5.0×10 -6 mol L -1 , 1.0×10 -7 mol L -1 , 2.0×10 -7 mol L -1 , 5.0×10 -7 mol L -1 , 5.0×10 -8 mol L -1 , 20 mg of flower-shaped Ag@β-CD was added respectively, and the absorbance was measured after oscillation for 1 h and 2 h respectively. Then, the adsorption amount of flower-shaped Ag@β-CD on methylene blue solutions of different concentrations after oscillation for 1 h and 2 h was calculated using Formula 1 and Formula 2 respectively, and the concentration and adsorption amount graphs after oscillation for 1 h and 2 h were plotted respectively.
[0069] Fig. 9 This is the adsorption amount of flower-shaped Ag@β-CD to methylene blue solutions of different concentrations after oscillation for 1 hour; Fig.10 Figure 2 shows the adsorption of flower-shaped Ag@β-CD on methylene blue solutions of different concentrations after oscillation for 2 h. It can be seen from the figure that the adsorption of flower-shaped Ag@β-CD changes slowly at the beginning with the increase of methylene blue concentration, whether it is oscillation for 1 h or 2 h. - 7 mol L -1 to 2.0×10 -6 mol L -1 When the adsorption amount changes, it increases from 2.0×10 -6 mol L -1 Later, the adsorption amount gradually tended to be constant, from which it can be judged that the concentration should be controlled at 2.0×10 -6 mol L -1 , because when the concentration reaches 2.0×10 -6 molL -1 When the adsorption amount tends to be constant, therefore, the concentration of 2.0×10 -6 mol L -1 Most suitable.
[0070] Example 6: Verification of the ability of Ag@β-CD fiber-based SERS substrate to enhance the Raman signal of dyes in printing and dyeing wastewater
[0071] 1. Methylene blue Raman spectrum and analysis: In Via laser confocal Raman spectrometer (INVIAREFLEX; Renishaw, UK) was used to analyze 1.0×10 -6 mol L -1 Methylene blue was used for Raman detection. Fig.11 This is the Raman detection image of methylene blue. It can be seen from the figure that the main characteristic peak of methylene blue is: 450cm -1 、480cm -1 、1039cm -1 、1073cm -1 、1153cm -1 、1179cm -1 、1396cm -1 、1624cm -1 Among them, the strongest peak is at 1624cm -1 The C-H stretching vibration characteristic peak is at 1396 cm -1 1073cm -1 1179cm -1 The peak at is C-N stretching vibration.
[0072] 2. Raman spectra and analysis of methylene blue with different concentrations enhanced by flower-like Ag@β-CD SERS substrate; Raman detection of methylene blue enhanced by flower-like Ag@β-CD SERS substrate. Fig.12 The Raman enhanced spectra of methylene blue with different concentrations on the flower-like Ag@β-CD SERS substrate are shown in the figure. As can be seen from the figure, as the concentration of methylene blue decreases, the intensity of the Raman peak also decreases. Most of the characteristic peaks of methylene blue with different concentrations appear in the same position. The detection concentration range of methylene blue enhanced by the flower-like Ag@β-CD SERS substrate is 1.0×10 -10 ~1.0×10 -4 mol L -1 In the detection concentration range, the flower-shaped Ag@β-CD SERS substrate can achieve the lowest concentration of 1.0×10 -10 mol L -1 Detection of methylene blue.
[0073] 3. Raman spectrum and analysis of Ag@β-CD fiber-based SERS substrate-enhanced methylene blue; methylene blue dye of different concentrations was dropped on the prepared flower-shaped Ag@β-CD fiber-based SERS substrate. The size of the flower-shaped Ag@β-CD fiber-based SERS substrate was 1cm×0.5cm. After adding one drop of methylene blue of different concentrations, the fiber substrate showed different shades of blue, which were arranged from top to bottom in order of the added concentration. Fig.13 The following are the pictures of Ag@β-CD fiber-based SERS substrate after adding different concentrations of methylene blue. From top to bottom, the concentration of methylene blue dye is 1.0×10 -6 mol L -1 , 1.0×10 -7 mol L -1 , 1.0×10 - 8 mol L -1 , 1.0×10 -9 mol L -1 , which facilitates the subsequent Raman detection of methylene blue using the flower-like Ag@β-CD fiber-based SERS substrate.
[0074] Fig.14 The concentration of Ag@β-CD fiber-based SERS substrate is 1.0×10 -6 mol L Raman enhanced spectrum of methylene blue. It can be seen from the figure that the characteristic peaks of methylene blue can be observed in many places in the Raman detection diagram of the flower-shaped Ag@β-CD fiber-based SERS substrate, indicating that the fiber base selected in this embodiment can be used as a substrate for Raman detection of methylene blue. The prepared flower-shaped Ag@β-CD fiber-based SERS substrate can achieve the adsorption of methylene blue. Compared with the Ag@β-CD SERS substrate detecting methylene blue, since the fiber base can also adsorb the dye, the flower-shaped Ag@β-CD fiber-based SERS substrate has a better SERS enhancement effect on methylene blue when detecting the same concentration of methylene blue.
[0075] In summary, flower-shaped Ag@β-CD can be used as a SERS substrate to detect methylene blue. Through in-depth analysis of the interaction between the SERS substrate and the methylene blue molecule, the results of flower-shaped Ag@β-CD adsorbing methylene blue at the same concentration and different time showed that the optimal adsorption time was 60 min; at different concentrations and the same time, the concentration of 2.0×10 -6 molL -1 The maximum adsorption amount can be obtained by oscillating for 1h. The flower-shaped Ag@β-CD is used as the SERS substrate to detect methylene blue. The characteristic peak intensity of methylene blue gradually weakens with the decrease of methylene blue concentration. The minimum concentration of methylene blue detected is 1.0×10 -10 molL -1The strongest characteristic peak of methylene blue detected by using flower-shaped Ag@β-CD as SERS substrate appears at 1624 cm -1 The flower-like Ag@β-CD fiber-based SERS substrate also obtained similar results. The above conclusions show that the flower-like Ag@β-CD fiber-based SERS substrate has potential application prospects in methylene blue detection, which provides a useful reference for further research and application of SERS technology in biochemistry, environmental protection and other aspects.
[0076] The present invention provides an Ag@β-cyclodextrin fiber-based SERS substrate and a preparation method thereof and a method for its application in the detection of printing and dyeing wastewater. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. An Ag@β-cyclodextrin fiber-based SERS substrate, characterized in that: The Ag@β-cyclodextrin fiber-based SERS substrate is constructed by attaching β-cyclodextrin-modified silver nanoparticles to the surface of a fiber material; wherein the silver nanoparticles are in a flower-like structure.
2. The Ag@β-cyclodextrin fiber-based SERS substrate according to claim 1, characterized in that: The Ag@β-cyclodextrin fiber-based SERS substrate is prepared by an ascorbic acid reduction method; the Ag source in the Ag@β-cyclodextrin fiber-based SERS substrate is silver nitrate.
3. The method for preparing the Ag@β-cyclodextrin fiber-based SERS substrate according to any one of claims 1 or 2, characterized in that: The specific steps include: S1. Cut and clean fiber materials; S2. The fiber material after washing in step S1 is fully immersed in the β-cyclodextrin solution; S3. The silver nitrate solution is added to the β-cyclodextrin solution containing the fiber material in step S2, and stirred to obtain a mixture solution; S4. Adding the ascorbic acid solution to the mixture solution of step S3, stirring and centrifugally drying to obtain the Ag@β-cyclodextrin fiber-based SERS substrate.
4. The preparation method according to claim 3, characterized in that: In step S2, the concentration of the β-cyclodextrin solution is 0.8 to 1.2 mmol L -1 .
5. The preparation method according to claim 3, characterized in that: In step S3, the concentration of the silver nitrate solution is 0.08-0.12 mmol L -1 .
6. The preparation method according to claim 3, characterized in that: In step S4, the concentration of the ascorbic acid solution is 0.08 to 0.12 mmol L -1 .
7. The preparation method according to claim 3, characterized in that: The volume ratio of the beta-cyclodextrin solution, the silver nitrate solution and the ascorbic acid solution is (8-12):1:
1.
8. Use of the Ag@β-cyclodextrin fiber-based SERS substrate according to any one of claims 1 or 2 in detecting printing and dyeing wastewater.
9. The use according to claim 8, characterized in that: The dyes in the printing and dyeing wastewater include methylene blue.
10. The use according to claim 8, characterized in that: The detection concentration range of the Ag@β-cyclodextrin fiber-based SERS substrate in printing and dyeing wastewater is 1.0×10 -10 ~1.0×10 -4 mol L -1 .