Antibacterial and antiviral degradation-oxidized chitosan cotton fabric as well as preparation method and application thereof
By mixing nitric acid and phosphoric acid with acid oxidation of chitosan and combining with cotton cellulose through esterification reaction, the problem of decreased softness and weakened antibacterial and antiviral activity when combined with cotton fabric is solved, and efficient antibacterial and antiviral activity is achieved Performance and durability.
Patent Information
- Application Number
- CN202411250475.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art has problems such as decreasing softness, weakening of antibacterial and antiviral activity and large steric hindrance when combining chitosan with cotton fabrics, resulting in poor antibacterial and antiviral performance.
Chitosan is selectively oxidized by mixed acid with nitric acid and phosphoric acid. After degradation, the oxidized chitosan is combined with the hydroxyl group of cotton cellulose through an esterification reaction to form stable chemical bonds and improve antibacterial and antiviral properties.
The antibacterial and antiviral properties were significantly improved. The antibacterial and antiviral degradation-oxidized chitosan cotton fabric prepared can have an antibacterial rate of Staphylococcus aureus and E. coli, and the inhibition rate of phage MS2 is as high as 99%. Maintain good biological activity after multiple washes.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of cotton fabric modification, and more specifically to an antibacterial and antiviral degradation-oxidation chitosan cotton fabric and a preparation method and application thereof. Background Art
[0002] Health problems caused by bacterial and viral infections have become one of the most serious threats to public health. In particular, the frequent outbreaks of coronavirus (COVID-19) in the world have had a huge and expanding impact on health systems, the economy, and society. Therefore, it is crucial to develop a new type of antibacterial and antiviral material to prevent cross-infection between bacteria and viruses.
[0003] Cotton, as a renewable natural material, has excellent physical properties due to its cellulose structure. Cotton fabric is one of the most widely used raw materials in the global textile industry. It is low-cost, soft, comfortable and breathable. These characteristics make cotton fabric widely used in making clothing, personal protective equipment and other daily necessities. However, the large surface area and good hygroscopicity of cotton fabrics also make it an ideal breeding ground for microorganisms. With the increasing demand for antibacterial and antiviral textiles, how to give cotton fabrics long-lasting and effective antibacterial and antiviral functions while maintaining the original excellent properties has become a technical problem that needs to be solved urgently in the textile field.
[0004] Chitosan is a natural polysaccharide derived from crustaceans, which has a wide range of biological activities due to its unique chemical structure. Chitosan not only has multiple biological functions such as antibacterial, antiviral, antioxidant, and anti-inflammatory, but is also considered to be a highly promising antibacterial agent due to its non-toxicity and good biocompatibility. However, chitosan still has some limitations in practical applications. First, chitosan has a large molecular weight, and direct application on cotton fabrics may cause the fabric to become less soft and harder. Secondly, if chitosan is degraded into low-molecular-weight chitosan oligosaccharides, although its solubility is improved, the reduction in amino content may weaken its antibacterial and antiviral activity. In addition, the lack of strong chemical bonding between chitosan and cotton fabrics is also one of the important factors affecting its long-term antibacterial and antiviral effects.
[0005] In order to solve the above problems, researchers proposed to treat chitosan by chemical modification to improve its binding force with cotton fabrics and antibacterial and antiviral activity. These chemical modification techniques can not only optimize the physical and chemical properties of chitosan, but also effectively enhance its application performance on cotton fabrics, so that the prepared antibacterial and antiviral cotton fabrics can still maintain their biological activity during long-term use, providing new ideas and technical support for the development of public health protection materials.
[0006] Prior art CN 105061637 A uses a concentrated nitric acid-concentrated phosphoric acid-sodium nitrite system to selectively oxidize part or all of the hydroxyl groups at the C6 position of chitosan into carboxyl groups to obtain water-soluble antibacterial monocarboxyl chitosan, and uses it for amide modification of silk fabrics to obtain monocarboxyl chitosan amide-modified silk fabrics. Prior art CN 108385391A dissolves macromolecular chitosan in an ionic liquid, precipitates it through anhydrous methanol to form porous chitosan, and then uses a concentrated nitric acid-concentrated phosphoric acid-sodium nitrite system to selectively oxidize the C6 hydroxyl group in the chitosan, and finally grafts it onto cashmere yarn through amide cross-linking bonds. Prior art CN109338724 A dissolves low-crystallinity chitosan in an ionic liquid, uses a nitric acid / concentrated phosphoric acid-sodium nitrite system to selectively oxidize the chitosan, and then grafts it onto the treated cotton fabric through an amide chemical reaction. The above prior art allows oxidized chitosan to react with cashmere fibers and the like to form an amide reaction. However, there is a steric hindrance problem in the amide reaction, resulting in an insufficient reaction.
[0007] The use of HNO3 / H3PO4-NaNO2 mixture as an oxidant to oxidize the primary hydroxyl groups of cellulose has become one of the effective ways to introduce carbonyl and carboxyl functions into polysaccharides, but in heterogeneous reactions, it leads to a large amount of hydrolysis of cellulose and a low yield of oxygen-containing fibers. In addition, there is no report on the direct grafting of oxidized chitosan onto cotton fabrics by esterification reaction. Summary of the invention
[0008] The present invention provides an antibacterial and antiviral degradation-oxidation chitosan cotton fabric to overcome the defects of the large steric hindrance of the amide reaction and the further limitation of the types of reactive fibers described in the prior art.
[0009] Another object of the present invention is to provide a method for preparing antibacterial and antiviral degradation-oxidation chitosan cotton fabric;
[0010] Another object of the present invention is to provide an application of antibacterial and antiviral degradation-oxidation chitosan cotton fabric.
[0011] In order to solve the above technical problems, the technical solution of the present invention is as follows:
[0012] A method for preparing antibacterial and antiviral degradation-oxidation chitosan cotton fabric comprises the following steps:
[0013] S1. Synthesis of degradable-oxidized chitosan: adding a mixed acid of nitric acid and phosphoric acid and sodium nitrite to chitosan, and reacting in an acidic environment to obtain degradable-oxidized chitosan;
[0014] S2. Preparation of impregnation solution: Sodium hypophosphite and degraded-oxidized chitosan are stirred and dissolved in water to obtain an impregnation solution;
[0015] S3, adding cotton fabric into the impregnation solution, stirring and then standing for impregnation, drying and then curing, thus obtaining antibacterial and antiviral degradation-oxidation chitosan cotton fabric.
[0016] Furthermore, the chitosan in S1 has a deacetylation degree greater than 95% and a viscosity of 100-200 mPa.s.
[0017] Furthermore, the carboxyl content of the degraded-oxidized chitosan in S1 is greater than 27%.
[0018] Furthermore, the mass volume ratio of the mixed acid of nitric acid and phosphoric acid to chitosan in S1 is 1.5-9 g / mL; and the reaction time is 2-8 h.
[0019] Preferably, the added amount of chitosan is 2 to 4 g.
[0020] Preferably, the added amount of chitosan is 3 g.
[0021] Preferably, the mass volume ratio of the mixed acid of nitric acid and phosphoric acid to chitosan is 6 g / mL.
[0022] Preferably, the reaction time is 6 hours.
[0023] Preferably, the mass of sodium nitrite is 0.9-1.7% of the volume of the mixed acid of nitric acid and phosphoric acid.
[0024] Preferably, the mass of sodium nitrite is 1.7% of the volume of the mixed acid of nitric acid and phosphoric acid.
[0025] Preferably, in the mixed acid of nitric acid and phosphoric acid, the volume ratio of nitric acid to phosphoric acid is 2:1.
[0026] Furthermore, in the impregnation solution obtained in S2, the mass concentration of sodium hypophosphite is 3% to 6%, and the mass concentration of degraded-oxidized chitosan is 4% to 8%.
[0027] Preferably, in the impregnation solution obtained in S2, the mass concentration of sodium hypophosphite is 6%, and the mass concentration of degraded-oxidized chitosan is 5%.
[0028] Furthermore, the mass concentration of cotton fabric in S3 is 4% to 8%, and the mass ratio of degraded-oxidized chitosan to cotton fabric is 1 to 2:1 to 2.
[0029] Preferably, the cotton fabric comprises selected industrially produced cotton fabric.
[0030] Preferably, the mass concentration of cotton fabric in S3 is 5%, and the mass ratio of degraded-oxidized chitosan to cotton fabric is 1:1.
[0031] Furthermore, the stirring time in S3 is 3 to 5 minutes, the immersion temperature is 70 to 90° C., and the immersion time is 1 to 2 hours; the drying conditions are: drying at 90 to 110° C. to constant weight; and curing at 140 to 160° C. for 3 to 5 minutes.
[0032] Preferably, the stirring time is 3 to 5 minutes.
[0033] Preferably, the dipping temperature is 80° C. and the dipping time is 1 min; the drying temperature is 105° C.; the curing temperature is 150° C. and the curing time is 3 min.
[0034] Preferably, the drying time is 2 to 3 hours.
[0035] Preferably, the drying time is 2.5 h.
[0036] Furthermore, the cotton fabric described in S3 is subjected to the following treatment before being added to the impregnation liquid: the cotton fabric is washed with a surfactant, impurities are removed with an ethanol aqueous solution, and the fabric is rinsed with water and then dried.
[0037] Preferably, the cotton fabric is washed with 1% sodium dodecyl sulfate at 60°C for 1 hour, then washed with 70% ethanol aqueous solution at 60°C to remove impurities, then rinsed with deionized water for 3 times, and finally dried at 80°C.
[0038] An antibacterial and antiviral degradation-oxidation chitosan cotton fabric is prepared by the preparation method of the antibacterial and antiviral degradation-oxidation chitosan cotton fabric.
[0039] An application of the antibacterial and antiviral degradation-oxidation chitosan cotton fabric is applied to the fields of papermaking, textile, medical treatment and food packaging.
[0040] The present invention adopts a HNO3 / H3PO4-NaNO2 mixture to selectively oxidize chitosan, while reducing its molecular weight and improving its water solubility, selectively oxidizing the C6-OH of chitosan to carboxyl groups, and the carboxyl groups can directly react with the hydroxyl groups of cotton cellulose, making it possible to graft the degraded and oxidized chitosan onto surface textiles through a one-step esterification reaction, avoiding the use of a cross-linking agent.
[0041] Under the action of nitric acid / phosphoric acid-sodium nitrite mixed system, the acidic environment first causes the long chain part to be cut by β-(1,4) glycosidic bond to form many fragments of different molecular weights. Then, after a series of elimination and dehydrogenation reactions, degraded-oxidized chitosan is finally formed. The reactions that occur are:
[0042]
[0043] The active site at the C-6 position of chitosan is selectively oxidized to a carboxyl group, which can undergo an esterification reaction with the hydroxyl group on the cotton fabric fiber to obtain chitosan reactive cotton fabric.
[0044] Different types of fiber materials show different reactivity during the reaction with chitosan or its derivatives due to their different chemical compositions and structures. For example, materials such as silk, cashmere yarn and cotton fabrics have different chemical structures (such as the types and numbers of chemical groups on the surface) and the morphology and structure of the fiber surface, which affect the occurrence of the reaction, resulting in uneven reaction or reduced reaction rate, thus affecting the modification effect.
[0045] The amide reaction is the process of combining the amino groups of chitosan with the carboxyl groups on the fiber surface. However, in practical applications, due to the limitations of the fiber surface structure (such as the dense arrangement of fibers or the complexity of the surface morphology), the reaction sites are easily hindered, making it difficult for the reaction to proceed fully. The steric hindrance limits the effective contact and combination of the reactants, resulting in low reaction efficiency and the performance of the reaction products is not as good as expected.
[0046] The hydroxyl group on the cotton fiber that participates in the esterification reaction is smaller than the amino group that reacts with the cashmere fiber in the amide reaction, and its chemical structure is simple, and the space requirement of the reaction site is low. At the same time, in the esterification reaction, the reaction between the hydroxyl group and the carboxyl group does not need to overcome the repulsive force caused by the strong polarity of the amino group, so the steric hindrance is small. And the reaction is more complete, which greatly improves the performance of the product.
[0047] The method of the invention improves the water solubility of chitosan and obtains reaction sites with hydroxyl groups of cotton fabric, and selectively controls the range of chitosan molecular weight and the amount of carboxyl content within a suitable oxidation reaction time, thereby obtaining water-soluble oxidized chitosan with the highest antibacterial and antiviral activity.
[0048] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0049] 1. Significantly improve the antibacterial and antiviral properties: The present invention grafts degraded-oxidized chitosan onto cotton fabric, so that the final product has extremely strong antibacterial and antiviral properties. The prepared antibacterial and antiviral degraded-oxidized chitosan cotton fabric has an inhibition rate of 100% against Staphylococcus aureus and Escherichia coli, and an inhibition rate of up to 99% against bacteriophage MS2. This shows that the material is very effective in fighting bacteria and viruses.
[0050] 2. Long-lasting antibacterial and antiviral activity: After 30 washes, the material still maintains a 100% inhibition rate against Staphylococcus aureus, an inhibition rate against Escherichia coli of more than 98%, and an inhibition rate against MS2 of more than 85%, indicating that the cotton fabric of the present invention has excellent durability and can still maintain its biological activity after long-term use and multiple washings.
[0051] 3. Strong chemical stability and binding force: Degraded-oxidized chitosan forms a stable chemical bond with the hydroxyl groups on cotton fabrics through esterification reaction, making the material not easy to fall off during use and showing good stability during the washing process. This binding force effectively ensures that the antibacterial and antiviral properties of cotton fabrics remain the same after multiple washings.
[0052] 4. Material properties are not affected: In the test of cellulose crystal structure, it was found that the introduction of degradation-oxidation chitosan reaction did not significantly change the original crystal structure of cotton fabric, indicating that the present invention not only gives cotton fabric antibacterial and antiviral functions, but also retains its good physical properties, such as softness and breathability. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 The scanning electron microscope spectra of chitosan and degraded-oxidized chitosan, cotton fabric and degraded-oxidized chitosan cotton fabric;
[0054] Figure 2 Fourier transform infrared spectra of chitosan and degraded-oxidized chitosan, cotton fabric and degraded-oxidized chitosan cotton fabric;
[0055] Figure 3 are spectra of X-ray photoelectron spectrometer, a~b are the general spectra of chitosan and degraded-oxidized chitosan, c~d are the C1s spectra of chitosan and degraded-oxidized chitosan, e~f are the C1s spectra of cotton fabric and degraded-oxidized chitosan cotton fabric;
[0056] Figure 4 X-ray diffraction spectra of cotton fabric and degraded-oxidized chitosan cotton fabric. DETAILED DESCRIPTION
[0057] The present invention is further described below in conjunction with the accompanying drawings and specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0058] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0059] Cotton fabric was purchased from a local textile store. Chitosan (DD>95%), sodium nitrite (99%), calcium acetate (99%), sodium hypophosphite monohydrate (99%), sodium hydroxide (99%), sodium dodecyl sulfate (AR) were purchased from Aladdin Chemical Reagent Co., Ltd. Nitric acid (AR), phosphoric acid (AR, 85%), and glacial acetic acid (99.5%) were purchased from Sinopharm Chemical Reagent Co., Ltd. LB broth, LB agar, Escherichia coli (ATCC8739), and Staphylococcus aureus (ATCC6538) were purchased from Qingdao Haibo Biotechnology Co., Ltd. (Qingdao, Shandong, China). MS2 bacteriophage (ATCC 15597-B1) was a gift from Fuzhou University. All chemicals were used without further purification.
[0060] Example 1
[0061] 1. A method for preparing an antibacterial and antiviral oxidized chitosan-cotton fabric, comprising the following steps:
[0062] 1) The cotton fabric was washed in a 70% ethanol aqueous solution at 60°C for 1 hour, followed by rinsing with deionized water for 3 times and finally dried at 80°C.
[0063] 2) Dissolve 3g of chitosan powder in a 1% glacial acetic acid solution by volume, stir at 80°C until completely dissolved, and then cool to 25°C for use; then add 18ml of a mixed acid of nitric acid and phosphoric acid in a volume ratio of 2:1, and then add 0.162g of NaNO2 and react at room temperature under a closed environment for 6 hours. After the reaction is completed, add 3 times the volume of anhydrous ethanol, filter, and wash until the solution is neutral. Then soak in anhydrous ethanol to remove the oxidant. After vacuum drying, water-soluble degradable-oxidized chitosan powder is obtained.
[0064] 3) Add 0.6 g of sodium hypophosphite and 0.5 g of water-soluble degradable-oxidized chitosan powder into 10 mL of deionized water, stir at 25° C. for 10 minutes, and mix well.
[0065] 4) Take 0.5 g of clean cotton fabric and soak it in the impregnation solution, stir it at room temperature for 4 minutes, and then soak it at 80°C for 1 hour. Then dry it in an oven at 105°C to constant weight, and finally cure it in an oven at 150°C for 3 minutes, wash it with deionized water and dry it to obtain the degraded-oxidized chitosan antibacterial and antiviral cotton fabric.
[0066] 2. Performance testing
[0067] Embodiment 2-3
[0068] The technical solutions of Examples 2 to 3 are similar to those of Example 1, and the specific differences are shown in Table 1.
[0069] Table 1 Different technical solutions of Examples 2 to 3
[0070] Example 2 Example 3 Chitosan dosage 2g 4g The quality of sodium nitrite 0.16g 0.3g Chitosan reaction time 2h 8h Sodium hypophosphite quality 0.3g 0.6g Degradation-oxidation chitosan quality 0.4g 0.8g Cotton fabric quality 0.8g 0.4g Cotton fabric stirring time 3min 5min Impregnation conditions 90℃ / 1h 70℃ / 2h Drying conditions 90℃ / 2h 110℃ / 3h Curing conditions 140℃ / 5min 160℃ / 3min
[0071] Comparative Examples 1 to 9
[0072] The technical solutions of Comparative Examples 1 to 9 are similar to those of Example 1, and the specific differences are shown in Table 2.
[0073] Table 2 Technical solutions of Comparative Examples 1 to 9
[0074]
[0075] “ / ” indicates the same as Example 1.
[0076] Physical and chemical properties test methods
[0077] 1. Scanning Electron Microscope (SEM)
[0078] The morphologies of chitosan, degraded-oxidized chitosan, cotton fabric and degraded-oxidized chitosan cotton fabric were analyzed by scanning electron microscopy (Zeiss geminisem 300, Germany).
[0079] 2. Fourier transform infrared spectroscopy (FTIR)
[0080] Chitosan and degraded-oxidized chitosan, cotton fabric and degraded-oxidized chitosan cotton fabric were analyzed by Fourier transform infrared spectrometer (Bruker VERTEX 70, Germany). -1 The spectral range was 332 scans with a resolution of 2 cm -1 .
[0081] 3. X-ray Photoelectron Spectrometer (XPS)
[0082] The surface chemical compositions of chitosan and degraded-oxidized chitosan, cotton fabric and degraded-oxidized chitosan cotton fabric were determined by XPS (Thermo Scientific K-Alpha, USA) with the energy step size set to 1.0 eV.
[0083] 4. X-ray diffractometer (XRD)
[0084] Data were collected using an X-ray diffractometer (XRD) (Ultima IV, Japan) with Ni filter and CuKα radiation, operating at 45 kV and 40 mA, with a continuous scan at an angular speed of 2° / min in the angular range of 5°≤2θ≤80°.
[0085] 5. Antibacterial analysis
[0086] The antibacterial performance of degraded-oxidized chitosan cotton fabric is expressed by the antibacterial rate, with Staphylococcus aureus and Escherichia coli as the test bacteria, referring to GB / T20944.3-2008. The bacteria were cultured in a shaker at 37°C for 18 hours until the bacteria concentration reached 10 9 CFU / mL, then diluted to 10 5 CFU / mL, used as inoculation solution for later use. Take cotton fabric and degraded-oxidized chitosan cotton fabric (on an absolute dry basis) respectively, and add them to a conical flask containing 10mL of inoculation solution. Incubate in a 37°C shaker for 1, 3, 6, 12, and 24 hours respectively. The incubated bacterial solution was diluted 10 times with PBS buffer, and 0.1mL was spread on the agar plate. Subsequently, the culture dish was cultured in an incubator at 37°C for 24 hours. Count the number of colonies on the plate and calculate the bacterial concentration of the conical flasks where different samples are located. Each group was repeated 3 times. The antibacterial rate calculation formula is as follows:
[0087]
[0088] Where:
[0089] Y——Inhibition rate of the sample
[0090] W——Concentration of viable bacteria in the conical flask after shaking contact with the control sample (CFU / mL)
[0091] Q—Concentration of viable bacteria in the conical flask after the sample is shaken and contacted (CFU / mL).
[0092] 6. Antiviral analysis
[0093] The antiviral properties of degraded-oxidized chitosan cotton fabrics were tested with bacteriophage MS2 as the test virus, referring to ISO 18184-2019. 0.5 mL of MS2 (10 6 PFU / mL) was dripped onto cotton fabric and degraded-oxidized chitosan cotton fabric (0.1 g). After incubation at 37°C for 1 h, the plaques of both fabrics were measured by double-layer plates to determine the MS2 concentration.
[0094] The formula for calculating the virus inhibition rate is as follows:
[0095]
[0096] Where:
[0097] A——Virus concentration in control sample
[0098] B——Virus concentration in the experimental sample
[0099] Results Analysis
[0100] (1) Scanning electron microscopy analysis
[0101] The chitosan and degraded-oxidized chitosan, cotton fabric and oxidized chitosan-cotton fabric prepared in Example 1 were analyzed by scanning electron microscope. The results are as follows: Figure 1 shown.
[0102] With original cotton fabric ( Figure 1 Compared with a), the surface of degraded-oxidized chitosan cotton fabric did not change much under low-power microscope, indicating that the degraded-oxidized chitosan was mainly coated on the fabric surface and did not occupy the fiber gap ( Figure 1 c). Under a high-power microscope, the surface of the original fabric fibers is smooth and neat ( Figure 1 b). In contrast, the surface of the modified fabric fiber becomes rougher ( Figure 1 d). Chitosan has a dense and flat surface ( Figure 1 e, g), while the degraded-oxidized chitosan showed a layered structure with granular particles, and oxidation caused a significant change in the surface morphology of chitosan ( Figure 1 f, h). This indicates that chitosan is depolymerized during the oxidative degradation process, resulting in the destruction of the crystal structure.
[0103] (2) Fourier transform infrared analysis
[0104] The chitosan and degraded-oxidized chitosan, cotton fabric and degraded-oxidized chitosan cotton fabric prepared in Example 1 were subjected to Fourier transform infrared spectroscopy analysis. The results are as follows: Figure 2 shown.
[0105] At 3429.81cm -1 and 3434.03cm -1 There is a strong and broad absorption peak at 1658.21 cm -1 The amide I absorption band is shown at 1599.3 cm -1 is the bending vibration peak of -NH. The degradation-oxidation chitosan is at 1752.89cm -1 The stretching vibration peak at 894.45 cm-1 can be attributed to the stretching vibration of the C=O double bond of the carboxyl group. -1 The vibration absorption bands at the β-pyranosidic bond and other positions showed some changes, indicating that after degradation and oxidation, the primary hydroxyl group at the C6 position of chitosan has been oxidized to a carboxyl group ( Figure 2 a). At the same time at 1376cm -1 、1062cm -1 and 890cm -1In addition to these characteristic peaks of cellulose, oxidized chitosan-cotton fabric also showed the characteristic peak position of carboxyl group, which indicated that the carboxyl group in oxidized chitosan and the hydroxyl group in cellulose underwent esterification reaction, that is, the degraded-oxidized chitosan had been successfully grafted onto cotton fabric ( Figure 2 b).
[0106] (3) X-ray Photoelectron Spectroscopy (XPS)
[0107] The degraded-oxidized chitosan and degraded-oxidized chitosan cotton fabric prepared in Example 1, as well as chitosan and untreated cotton fabric were subjected to X-ray photoelectron spectroscopy analysis. The spectrum is shown in FIG. Figure 3 shown.
[0108] In the overall spectrum, both chitosan and degraded-oxidized chitosan showed peaks of C1S, O 1S, and N1S ( Figure 3 a). However, there are some differences in the contents of O and C between the samples before and after modification. In comparison, the content of O significantly increased from 25.84% to 42.54% (Table 3), and the content of C=O also increased from 13.31% to 22.8% (Table 4). At the same time, the cotton fabric and the degraded-oxidized chitosan cotton fabric were also characterized and analyzed. In the overall spectrum, the degraded-oxidized chitosan cotton fabric showed the N element ( Figure 3 b), which is not found in the original cotton fabric, indicating that the degraded-oxidized chitosan has been grafted onto the cotton fabric. In the C1s spectrum of the degraded-oxidized chitosan, the intensity of the C=O peak is significantly increased compared with that of the untreated chitosan ( Figure 3 c, d). The above conclusions indicate that the hydroxyl group at the C-6 position of chitosan has been successfully oxidized to a carboxyl group. The change in the CO peak also indicates the change in the chitosan structure during degradation and oxidation, which is usually accompanied by the oxidation reaction. The C1 s high-resolution XPS spectra of the two cotton fabric samples are shown in Figures e to f, respectively. The cotton fabric has three peaks at 283.3, 285 and 285.9 eV, which are CC, CH and C=O, respectively, while the oxidized chitosan-cotton fabric has four peaks at 283.5, 284.9, 285.6 and 286.8 eV, which are attributed to CC, CH, CN and C=O, respectively. These results prove the successful modification of cotton fabric by degraded-oxidized chitosan.
[0109] Table 3 Elemental composition of chitosan and degraded-oxidized chitosan
[0110]
[0111] Table 4 Functional group composition of cotton fabric and degraded-oxidized chitosan cotton fabric
[0112]
[0113] (4) X-ray diffraction (XRD)
[0114] The cotton fabric and oxidized chitosan-cotton fabric obtained in Example 1 were subjected to X-ray diffraction analysis. The results are as follows: Figure 4 shown.
[0115] Cotton fabric and oxidized chitosan-cotton fabric have diffraction peaks at 14.8°, 16.9°, 22.7° and 34.3°, corresponding to the four crystal planes (110)(110), (200) and (004), respectively. These crystal planes are the characteristic crystal planes of cellulose I. The diffraction peaks of the original fabric and the modified fabric are almost identical, indicating that the introduction of degradation-oxidation chitosan does not change the crystalline form of cellulose during the reaction process. At the same time, the crystallinity of the unmodified cotton fabric is 58%, and the crystallinity of the oxidized chitosan-cotton fabric is 55%. The results show that the structure of cotton fabric cellulose is not significantly affected by the modification process, and the crystallinity is largely retained.
[0116] (5) Analysis of carboxyl content
[0117] As shown in Table 5, Example 1 can obtain a higher carboxyl content than Comparative Example 1. As shown in Comparative Example 1, the amount of chitosan used has a certain influence on the carboxyl content. As shown in Comparative Example 2, the oxidation time of chitosan has a significant influence on the carboxyl content, and too little reaction time leads to a significant reduction in the carboxyl content. As shown in Comparative Example 3, when the reaction time is less than 2 hours, even if the amount of chitosan is reduced, the carboxyl content of the degraded-oxidized chitosan cannot be increased. As shown in Comparative Example 4, when the reaction time is greater than 8 hours, too much time leads to side reactions, and even if the amount of chitosan is increased, the carboxyl content of the degraded-oxidized chitosan cannot be increased.
[0118] Table 5 Carboxyl content of degraded-oxidized chitosan
[0119]
[0120] At the same time, according to Table 6, it is found through Comparative Examples 2 and 3 that the molecular weight of chitosan drops sharply before 2 hours of reaction, which may be due to the cleavage of the β-(1,4) glycosidic bond, which causes the molecular chain to initially break into shorter ones. However, the molecular weight of Comparative Example 4 increases slightly after a certain period of time compared with Example 1. The physical structure of chitosan expands due to severe degradation, resulting in fragments of various molecular weights, and the side reaction between the amino groups of chitosan molecules may be the reason for the slight increase in molecular weight.
[0121] Table 6 Molecular weight of degraded-oxidized chitosan
[0122]
[0123] (6) Analysis of antibacterial and antiviral properties
[0124] As can be seen from Table 7, the antibacterial and antiviral degradation-oxidized chitosan cotton fabric prepared in Example 1 can achieve an inhibition rate of 100% against two types of bacteria. This shows that oxidized chitosan-cotton fabric has a very high antibacterial activity. This result can be explained by the interaction between the positive charge on chitosan and the negative charge in the cells of bacterial microorganisms, resulting in leakage of intracellular substances. On the other hand, it is the result of the interaction between the positive charge of chitosan and the DNA of microorganisms, which inhibits the synthesis of RNA and protein and the antibacterial and antiviral activity. The cell wall of Gram-negative bacteria is more complex but thinner than that of Gram-positive bacteria. It contains a semipermeable membrane located on the peptidoglycan layer, which inhibits certain antibiotics from entering the cell, so the antibacterial effect on Staphylococcus aureus is generally higher than that on Escherichia coli.
[0125] Table 7 Antibacterial and antiviral properties
[0126]
[0127] Bacteriophage MS2 is a non-enveloped positive-strand RNA virus. Due to its icosahedral structure and small size, it is a potential alternative to SARS-CoV-2, influenza virus, norovirus, etc. Chitosan is able to kill viruses by binding to proteins in the viral capsid and causing structural damage to the virus. As shown in Table 7, the oxidized chitosan antibacterial and antiviral cotton fabric can reduce the viral load by 99% after 1 hour of contact, indicating that the oxidized chitosan-cotton fabric has good antiviral properties.
[0128] As can be seen from Comparative Example 5, the concentration of the catalyst sodium hypophosphite affects the preparation process. Increasing the catalyst concentration will lead to over-catalysis, which will reduce the antibacterial and antiviral results of cotton fabrics, indicating that the appropriate catalyst concentration can improve the antibacterial activity of cotton fabrics. As can be seen from Comparative Example 6, the concentration of degraded-oxidized chitosan is a key factor in the preparation process. Increasing the mass concentration of the antibacterial and antiviral agent chitosan leads to heterogeneity in the material, affects the efficiency of the esterification reaction, and does not improve its antibacterial and antiviral effect. As can be seen from Comparative Example 7, the amount of cotton fabric also affects the performance of the final product. Reducing the proportion of the material directly affects the uniformity of the reaction and does not improve the antibacterial and antiviral effect. As can be seen from Comparative Example 9, while lowering the drying temperature, the drying time is extended. However, the antibacterial and antiviral ability of the final product is still reduced. Temperature has an important influence on the rate and product yield of the esterification reaction. Too low a drying temperature will lead to a slow reaction rate, and too high a drying temperature will increase side reactions and product losses. Selecting the most suitable sample drying temperature can obtain the final product in the shortest time under the premise of ensuring the antibacterial and antiviral effect.
[0129] The antibacterial and antiviral degraded-oxidized chitosan cotton fabric prepared in Example 1 of the present invention has the highest antibacterial and antiviral activity. The results show that cross-linking degraded-oxidized chitosan on cotton fabric through esterification is an effective method to obtain cotton fabric with excellent antibacterial properties.
[0130] Table 824h antibacterial performance
[0131]
[0132] Note: 100% means the antibacterial rate is greater than or equal to 99.999%.
[0133] The results in Table 8 show that the degradation-oxidation chitosan cotton fabric has a strong inhibitory effect on the growth of bacteria, and the inhibition rate of Staphylococcus aureus and Escherichia coli can reach almost 100% in 24 hours. In this test, the inhibition of Staphylococcus aureus is better than that of Escherichia coli. This verifies the feasibility of oxidized chitosan antibacterial and antiviral cotton fabric as an antibacterial and antiviral textile material.
[0134] (7) Antibacterial and antiviral durability analysis
[0135] The antibacterial and antiviral durability of the degraded-oxidized chitosan cotton fabric prepared in Example 1 was evaluated every 10 washing cycles.
[0136] Table 9 Antibacterial durability and antiviral durability
[0137]
[0138] Note: A result showing 100% means the antibacterial rate is greater than or equal to 99.999%.
[0139] As shown in Table 9, after 30 washing cycles, the inhibition rate against Staphylococcus aureus remained 100%, the inhibition rate against Escherichia coli was above 98%, and the inhibition rate against bacteriophage MS2 was above 85%. The results show that the antibacterial and antiviral activities of the degraded-oxidized chitosan cotton fabric of the present invention are long-lasting, and the degraded-oxidized chitosan and the cotton fabric are chemically connected to cellulose through an ester bond, and are stable to the shear force encountered in the washing system.
[0140] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing antibacterial and antiviral degradation-oxidation chitosan cotton fabric, characterized in that: The following steps are involved: S1. Synthesis of degradable-oxidized chitosan: adding a mixed acid of nitric acid and phosphoric acid and sodium nitrite to chitosan for reaction to obtain degradable-oxidized chitosan; S2. Preparation of impregnation solution: Sodium hypophosphite and degraded-oxidized chitosan are stirred and dissolved in water to obtain an impregnation solution; S3, adding cotton fabric into the impregnation solution, stirring and then standing for impregnation, drying and then curing, thus obtaining antibacterial and antiviral degradation-oxidation chitosan cotton fabric.
2. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: The chitosan in S1 has a deacetylation degree greater than 95% and a viscosity of 100-200 mPa.s.
3. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: The carboxyl content of the degraded-oxidized chitosan in S1 is greater than 27%.
4. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: The mass volume ratio of the mixed acid of nitric acid and phosphoric acid to chitosan in S1 is 1.5-9 g / mL; and the reaction time is 2-8 h.
5. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: In the impregnation solution obtained in S2, the mass concentration of sodium hypophosphite is 3% to 6%, and the mass concentration of degraded-oxidized chitosan is 4% to 8%.
6. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: The mass concentration of cotton fabric in S3 is 4% to 8%, and the mass ratio of degraded-oxidized chitosan to cotton fabric is 1 to 2:1 to 2.
7. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: The stirring time in S3 is 3 to 5 minutes, the immersion temperature is 70 to 90° C., and the immersion time is 1 to 2 hours; the drying conditions are: drying at 90 to 110° C. to constant weight; and curing at 140 to 160° C. for 3 to 5 minutes.
8. The method for preparing the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 1, characterized in that: The cotton fabric described in S3 is subjected to the following treatment before being added to the impregnation solution: the cotton fabric is cleaned with a surfactant, impurities are removed with an ethanol aqueous solution, the fabric is rinsed with water, and then dried.
9. An antibacterial and antiviral degradation-oxidation chitosan cotton fabric, characterized in that: The antibacterial and antiviral degradable-oxidized chitosan cotton fabric is prepared by the preparation method of any one of claims 1 to 8.
10. An application of the antibacterial and antiviral degradation-oxidation chitosan cotton fabric according to claim 9, characterized in that: Used in papermaking, textile, medical and food packaging fields.