Natural nanofiber grafted polylysine as well as preparation method and application thereof

By connecting natural nanofibers with polylysine, natural nanofiber grafted polylysine with antibacterial properties is prepared, which solves the problems of degraded mechanical properties and insufficient antibacterial properties of silk fibroprotein materials, and realizes fresh preservation in food and Widely used in the field of biomedicine.

CN119083184APending Publication Date: 2024-12-06ZHEJIANG SCI-TECH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411188438.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The regenerated silk fibroprotein material has a decline in mechanical properties and lacks antibacterial properties, which limits its application areas.

Method used

By connecting natural nanofibers and polylysine through amide bonds, natural nanofiber graft polylysine is prepared to improve its antibacterial properties, and ensure its biocompatibility and drug resistance through specific preparation methods. .

Benefits of technology

It has achieved the improvement of antibacterial properties of natural nanofibers, expanded its application prospects in the fields of food preservation and biomedicine, while maintaining biocompatibility and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083184A_ABST
    Figure CN119083184A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional materials, and particularly relates to natural nanofiber grafted polylysine as well as a preparation method and application thereof. According to the invention, the natural nanofiber is modified with the polylysine with an antibacterial function to obtain the natural nanofiber grafted polylysine, and the natural nanofiber grafted polylysine has good antibacterial property and biocompatibility, is not easy to generate drug resistance, has no side effect on a human body, and has a good application prospect in the biomedical field. The natural nanofiber grafted polylysine provided by the invention can be made into a natural nanofiber grafted polylysine biological membrane, a natural nanofiber grafted polylysine hydrogel, a natural nanofiber grafted polylysine sponge material and the like, and is applied to the fields of food preservation, biological medicine and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and specifically relates to a natural nanofiber grafted polylysine and a preparation method and application thereof. Background Art

[0002] Silk fibroin is composed of multi-component amino acids. The presence of amphoteric amino and carboxyl groups in the skeleton is conducive to its combination with polymers. It has the advantages of easy modification, good biocompatibility, negligible immunogenicity and multiple biological activities. It is widely used in fibers, films, microspheres and porous matrices.

[0003] At present, the mechanical properties of regenerated silk protein materials have declined. The reason is that the regeneration preparation process destroys the highly ordered nanofiber structure of silk fibers at the microscopic scale. Silk nanofibers are fibers with a diameter of nanometers obtained by peeling off silk fibers. They retain the structure of silk fibers at the microscopic scale as well as the excellent mechanical properties of silk fibers.

[0004] However, silk fiber also has many shortcomings in performance, such as the lack of antibacterial properties, which limits its application areas. Summary of the invention

[0005] The purpose of the present invention is to provide a natural nanofiber grafted polylysine and a preparation method and application thereof. The natural nanofiber grafted polylysine provided by the present invention has good antibacterial properties.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a natural nanofiber grafted with polylysine, comprising natural nanofiber and polylysine connected with the natural nanofiber through amide bonds.

[0008] Preferably, the natural nanofiber grafted polylysine is natural nanofiber grafted ε-polylysine or natural nanofiber grafted α-polylysine.

[0009] Preferably, the number average molecular weight of the natural nanofiber grafted polylysine is 20 to 500 KDa.

[0010] The present invention also provides a method for preparing the natural nanofiber grafted polylysine described in the above scheme, comprising the following steps:

[0011] (1) mixing natural fibers, alkali, urea and water to obtain a natural nanofiber suspension;

[0012] (2) The natural nanofiber suspension is mixed with a crosslinking agent and polylysine for grafting reaction to obtain a natural nanofiber grafted polylysine suspension; the mass ratio of natural nanofibers to polylysine in the natural nanofiber suspension is not less than 5:1; the molar ratio of carboxyl groups of natural nanofibers to crosslinking agent in the natural nanofiber suspension is 1:0.1 to 1.0.

[0013] Preferably, the polylysine includes one or more of ε-polylysine and α-polylysine; and the number average molecular weight of the polylysine is less than 5000 Da.

[0014] Preferably, the temperature of the grafting reaction is -15 to 10° C., and the insulation time is 2 to 8 hours.

[0015] The present invention also provides the use of the natural nanofiber grafted polylysine described in the above scheme or the natural nanofiber grafted polylysine obtained by the preparation method described in the above scheme as an antibacterial material.

[0016] The present invention also provides a method for preparing a natural nanofiber grafted polylysine biofilm, comprising the following steps:

[0017] The natural nanofiber grafted polylysine suspension is dried to form a film to obtain a natural nanofiber grafted polylysine biofilm; the natural nanofiber grafted polylysine suspension is the natural nanofiber grafted polylysine suspension obtained by the preparation method described in the above scheme.

[0018] The present invention also provides a method for preparing a natural nanofiber grafted polylysine hydrogel, comprising the following steps:

[0019] The natural nanofiber grafted polylysine suspension is stirred and mixed with a crosslinking agent and then allowed to stand to form a gel to obtain a natural nanofiber grafted polylysine hydrogel; the natural nanofiber grafted polylysine suspension is the natural nanofiber grafted polylysine suspension obtained by the preparation method described in the above scheme.

[0020] The present invention also provides a method for preparing a natural nanofiber grafted polylysine sponge material, comprising the following steps:

[0021] The natural nanofiber grafted polylysine suspension is freeze-dried to obtain a natural nanofiber grafted polylysine sponge material; the natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method described in the above scheme.

[0022] The present invention provides a natural nanofiber grafted with polylysine. The present invention combines the carboxyl group on the natural nanofiber with the amino group on the polylysine, and utilizes the amide bond reaction to prepare the natural nanofiber modified with polylysine as a functional antibacterial material, thereby improving the antibacterial ability of the natural nanofiber and the antibacterial ability of the polymer based on the natural nanofiber. The natural nanofiber grafted with polylysine prepared by the present invention contains a large number of amino groups, and the presence of the amino group is conducive to its combination with polymers or drugs, and can be easily processed into films, sponges, gels, etc. The present invention modifies polylysine with antibacterial function onto natural nanofibers to obtain natural nanofiber grafted with polylysine, which has good antibacterial properties, is not easy to produce drug resistance, has no side effects on the human body, and has good application prospects in the fields of food preservation and biomedicine.

[0023] The present invention also provides a method for preparing the natural nanofiber grafted polylysine described in the above scheme. The present invention uses polylysine as a raw material, and grafts it onto natural nanofibers through a crosslinking system according to a certain dosage ratio to prepare the natural nanofiber grafted polylysine, which has good antibacterial and biocompatibility, is not easy to produce drug resistance, and has broad application prospects.

[0024] The present invention also provides the use of the natural nanofiber grafted polylysine described in the above scheme or the natural nanofiber grafted polylysine obtained by the preparation method described in the above scheme as an antibacterial material. The natural nanofiber grafted polylysine provided by the present invention has good antibacterial properties and biocompatibility, is not easy to produce drug resistance, and has broad application prospects in the fields of food preservation and biomedicine.

[0025] The present invention also provides a method for preparing a natural nanofiber grafted polylysine biofilm. The present invention adopts the natural nanofiber grafted polylysine suspension of the above scheme and obtains the biofilm by drying. The preparation method provided by the present invention has simple steps, convenient operation and high feasibility.

[0026] The present invention also provides a method for preparing a natural nanofiber grafted polylysine hydrogel. The present invention utilizes the natural nanofiber grafted polylysine suspension of the above scheme to obtain a hydrogel by further gelation. The preparation method provided by the present invention has simple steps and is easy to operate.

[0027] The present invention also provides a method for preparing a natural nanofiber grafted polylysine sponge material. The present invention freeze-dries the natural nanofiber grafted polylysine suspension of the above scheme to obtain a natural nanofiber grafted polylysine sponge material. The preparation method provided by the present invention has simple steps, low cost and good economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 The schematic diagram of the synthesis of natural nanofiber grafted with ε-polylysine of the present invention;

[0030] Figure 2 The schematic diagram of the synthesis of natural nanofiber grafted with α-polylysine of the present invention;

[0031] Figure 3 The actual picture (left) and the Tyndall effect picture (right) of the natural nanofiber suspension and the natural nanofiber grafted polylysine suspension prepared in Example 1 and Example 2;

[0032] Figure 4 Zeta potential diagrams of the natural nanofiber suspension, natural nanofiber grafted polylysine suspension and polylysine solution prepared in Example 1 and Example 2;

[0033] Figure 5 SEM images of natural nanofibers (left) and natural nanofibers grafted with polylysine (right) prepared in Example 1 and Example 2;

[0034] Figure 6 The antibacterial results of the natural nanofibers and natural nanofibers grafted with polylysine prepared in Example 1 and Example 2 are shown;

[0035] Figure 7 This is a diagram showing the effects of natural nanofibers prepared in Example 1 and Example 2 and natural nanofibers grafted with polylysine for food preservation. DETAILED DESCRIPTION

[0036] The invention provides a natural nanofiber grafted with polylysine, comprising natural nanofiber and polylysine connected with the natural nanofiber through amide bonds.

[0037] In the present invention, the natural nanofiber grafted polylysine is preferably natural nanofiber grafted ε-polylysine or natural nanofiber grafted α-polylysine.

[0038] In the present invention, the number average molecular weight of the natural nanofiber grafted with polylysine is preferably 20 to 500 KDa, more preferably 50 to 400 KDa, and further preferably 100 to 200 KDa.

[0039] The present invention also provides a method for preparing the natural nanofiber grafted polylysine described in the above scheme, comprising the following steps:

[0040] (1) mixing natural fibers, alkali, urea and water to obtain a natural nanofiber suspension;

[0041] (2) The natural nanofiber suspension is mixed with a crosslinking agent and polylysine to carry out a grafting reaction to obtain a natural nanofiber grafted polylysine suspension.

[0042] The present invention mixes natural fibers, alkali, urea and water (referred to as the first mixing) to obtain a natural nanofiber suspension. In the present invention, the natural fibers are preferably natural silk fibers; the diameter of the natural fibers is preferably 10 to 1000 nm, more preferably 30 to 300 nm.

[0043] In the present invention, the base is preferably a strong base; the strong base preferably includes one or more of an inorganic strong base and an organic strong base; the inorganic strong base preferably includes one or both of sodium hydroxide and potassium hydroxide; the organic strong base preferably includes one or both of sodium methoxide and sodium ethoxide.

[0044] In the present invention, the water is preferably deionized water. The present invention utilizes alkali solution to peel off the natural fibers, and then disperses them in deionized water to form a suspension.

[0045] In the present invention, the mass ratio of the alkali to urea is preferably 5-10:10-18, more preferably 5-8:10-15; the mass ratio of the urea to water is preferably 10-18:72-85, more preferably 10-15:77-85; the ratio of the mass of the natural fiber to the total mass of the alkali, urea and water is preferably 1-5:100, more preferably 2-4:100.

[0046] In the present invention, the alkali and urea are preferably frozen before the first mixing; the freezing temperature is preferably -45 to -10°C, more preferably -25 to -15°C, and the insulation time is preferably 8 to 48 hours, more preferably 20 to 36 hours.

[0047] In the present invention, the first mixing is preferably: stirring and mixing the natural fiber, strong alkali, urea and water, followed by first centrifugation, ultrasound, second centrifugation, first freeze drying and third centrifugation.

[0048] In the present invention, the stirring and mixing is preferably: stirring for 10 to 20 minutes every 12 hours; the total time of the stirring and mixing is preferably 40 to 54 hours, more preferably 48 hours.

[0049] In the present invention, the rotation speed of the first centrifugation is preferably 5000-10000 rpm, more preferably 6000-9000 rpm, further preferably 7000-8000 rpm, and the centrifugation time is preferably 8-20 min, more preferably 10-15 min.

[0050] In the present invention, the power of the ultrasound is preferably 24-40% of the rated power, more preferably 30-34%, and the time is preferably 20-35 minutes, more preferably 25-30 minutes.

[0051] In the present invention, the rotation speed of the second centrifugation is preferably 5000-8000 rpm, more preferably 6000-7000 rpm, and the centrifugation time is preferably 5-20 min, more preferably 8-15 min. In the present invention, the sediment at the bottom is removed by the second centrifugation to obtain an intermediate suspension.

[0052] In the present invention, the temperature of the first freeze-drying is preferably -45°C to -10°C, more preferably -25°C to -15°C, and the insulation time is preferably 8 to 48 hours, more preferably 20 to 36 hours.

[0053] In the present invention, the rotation speed of the third centrifugation is preferably 5000-8000 rpm, more preferably 6000-7000 rpm, and the centrifugation time is preferably 5-20 min, more preferably 10-15 min.

[0054] After obtaining the natural nanofiber suspension, the present invention mixes the natural nanofiber suspension with a crosslinking agent and polylysine (referred to as the first mixing) for grafting reaction to obtain a natural nanofiber grafted polylysine suspension. In the present invention, the crosslinking agent preferably includes one or more of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide system, horseradish peroxidase and hydrogen peroxide system, and genipin. The present invention grafts polylysine onto natural nanofibers through a crosslinking agent, thereby improving the antibacterial properties of natural nanofibers.

[0055] In the present invention, the polylysine preferably includes one or more of ε-polylysine and α-polylysine; the ε-polylysine is preferably ε-polylysine obtained by biological fermentation of Streptococcus albus; the number average molecular weight of the polylysine is preferably less than 5000Da, more preferably less than 4500Da.

[0056] In the present invention, the mass ratio of natural nanofibers to polylysine in the natural nanofiber suspension is preferably not less than 5:1, more preferably 5:0.1-1, and further preferably 5:0.3-0.7.

[0057] In the present invention, the molar ratio of the carboxyl groups of the natural nanofibers to the crosslinking agent in the natural nanofiber suspension is preferably 1:0.1 to 1.0, and more preferably 1:0.4 to 0.9.

[0058] In the present invention, the first mixing is preferably stirring; the temperature of the first mixing is preferably 0 to 30° C., more preferably 15 to 25° C., and the mixing time is preferably 20 to 40 min, more preferably 25 to 38 min.

[0059] In the present invention, the first mixing is more preferably: premixing the natural nanofiber suspension with a crosslinking agent to obtain a premixed solution, configuring polylysine to form a polylysine aqueous solution, and then mixing the premixed solution and the polylysine aqueous solution.

[0060] In the present invention, the temperature of the grafting reaction is preferably -15 to 10°C, more preferably -10 to 5°C, and the insulation time is preferably 2 to 8 hours, more preferably 3 to 5 hours.

[0061] In the present invention, after the grafting reaction, the obtained product is preferably post-treated; the post-treatment is preferably: dialyzing the obtained product of the grafting reaction with deionized water and then freeze-drying it.

[0062] In the present invention, the molecular weight cut-off of the dialysis is preferably greater than 5000 Da, more preferably greater than 5500 Da.

[0063] In the present invention, the freeze-drying temperature is preferably -45 to -10°C, more preferably -25 to -15°C, and the insulation time is preferably 8 to 48 hours, more preferably 20 to 36 hours.

[0064] The present invention also provides the use of the natural nanofiber grafted polylysine described in the above scheme or the natural nanofiber grafted polylysine obtained by the preparation method described in the above scheme as an antibacterial material.

[0065] The natural nanofiber grafted polylysine provided by the invention can be used to prepare biological materials such as natural nanofiber grafted polylysine biofilm, natural nanofiber grafted polylysine hydrogel or natural nanofiber grafted polylysine sponge material.

[0066] The present invention also provides a method for preparing a natural nanofiber grafted polylysine biofilm, comprising the following steps: drying a natural nanofiber grafted polylysine suspension into a film to obtain a natural nanofiber grafted polylysine biofilm; the natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method described in the above scheme.

[0067] In the present invention, the drying film is preferably drying after coating; the drying is preferably baking; the drying temperature is preferably 45-70°C, more preferably 55-65°C, and the insulation time is preferably 4-10h, more preferably 5-7h.

[0068] The present invention also provides a method for preparing a natural nanofiber grafted polylysine hydrogel, comprising the following steps: stirring and mixing a natural nanofiber grafted polylysine suspension with a crosslinking agent and then standing to form a gel to obtain a natural nanofiber grafted polylysine hydrogel; the natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method described in the above scheme.

[0069] In the present invention, the cross-linking agent preferably includes one or more of horseradish peroxidase and hydrogen peroxide system, genipin, glutaraldehyde, tyrosinase, transglutaminase, lysine oxidase and horseradish peroxidase.

[0070] In the present invention, the volume ratio of the natural nanofiber grafted polylysine suspension to the cross-linking agent is preferably 10:2-9, more preferably 10:4-6.

[0071] In the present invention, the step of placing the mixture into a mold before standing still preferably further comprises: placing the mixture obtained by stirring and mixing into a mold.

[0072] In the present invention, the standing temperature is preferably room temperature.

[0073] The present invention also provides a method for preparing a natural nanofiber grafted polylysine sponge material, comprising the following steps: freeze-drying a natural nanofiber grafted polylysine suspension (referred to as the second freeze-drying) to obtain a natural nanofiber grafted polylysine sponge material; the natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method described in the above scheme.

[0074] In the present invention, the natural nanofiber grafted polylysine suspension is preferably pretreated before the second freeze-drying; the pretreatment is preferably freezing; the freezing temperature is preferably -20 to -80°C, more preferably -20 to -40°C, and the insulation time is preferably 4 to 18 hours, more preferably 10 to 14 hours.

[0075] In the present invention, the temperature of the second freeze-drying is preferably -45 to -10°C, more preferably -25 to -15°C, and the insulation time is preferably 8 to 48 hours, more preferably 20 to 36 hours.

[0076] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0077] In a specific embodiment of the present invention, the 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide and N-hydroxysuccinimide were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0078] Example 1

[0079] This example prepares a natural nanofiber grafted polylysine - natural silk nanofiber grafted ε-polylysine biofilm, the reaction mechanism is as follows Figure 1 shown.

[0080] (1) Preparation of silk nanofiber suspension: Weigh 2 g of silk nanofiber and add it to a frozen sodium hydroxide / urea aqueous solution, wherein the mass ratio of sodium hydroxide to urea is 7:12, the mass ratio of urea to water is 12:81, and the ratio of the mass of natural fiber to the total mass of sodium hydroxide, urea and water is 1:50; stir with a mechanical stirrer for 10 min every 12 h, centrifuge at 8000 rpm for 10 min after 48 h until the pH is <8, and then ultrasonically crush with an ultrasonic crusher for 30 min, and centrifuge at 8000 rpm for 15 min to remove the bottom precipitate to obtain an intermediate suspension; freeze-dry the intermediate suspension at -45°C in a freeze dryer for 18 h to obtain freeze-dried silk nanofibers; add the freeze-dried silk nanofibers (10-1000 nm) to deionized water and centrifuge at 8000 rpm for 10 min to obtain a silk nanofiber suspension, wherein the concentration of the silk nanofibers is 3 wt%.

[0081] (2) Preparation of a natural silk nanofiber grafted ε-polylysine suspension: Add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide in an amount of 150 μL / mL to the silk nanofiber suspension prepared in step (1) to obtain a premixed solution; then add N-hydroxysuccinimide in an amount of 75 μL / mL to the premixed solution, and stir at low temperature for 30 min to obtain a mixed solution; then, add ε-polylysine (number average molecular weight less than 5000 Da) accounting for 5% of the mass of the silk nanofiber to the mixed solution, stir at low temperature at 4°C for 35 min, and then carry out a grafting reaction at 4°C for 6 h. After the reaction is completed, a natural silk nanofiber grafted ε-polylysine suspension is obtained.

[0082] (3) Preparation of natural silk nanofiber grafted ε-polylysine biofilm: The natural silk nanofiber grafted ε-polylysine suspension prepared in step (2) is dried at 60°C and kept warm for 8 hours to obtain a natural silk nanofiber grafted ε-polylysine biofilm material, which can be used in food preservation and other fields.

[0083] Example 2

[0084] This embodiment prepares a natural nanofiber grafted polylysine, that is, a natural silk nanofiber grafted ε-polylysine sponge material.

[0085] (1) Preparation of silk nanofiber suspension: freeze-dried silk nanofibers (30-300 nm) were added to deionized water and centrifuged at 7000 rpm for 10 minutes to prepare a silk nanofiber suspension with a silk nanofiber concentration of 3 wt%.

[0086] (2) Preparation of a natural silk nanofiber grafted ε-polylysine suspension: Add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide in an amount of 150 μL / mL to the silk nanofiber suspension prepared in step (1) to obtain a premixed solution; then add N-hydroxysuccinimide in an amount of 75 μL / mL to the premixed solution, stir at low temperature for 30 min, and obtain a mixed solution; subsequently, add ε-polylysine (number average molecular weight less than 5000 Da) accounting for 5% of the mass of the silk nanofiber to the mixed solution, stir at low temperature at 0°C for 30 min, and perform grafting reaction at 0°C for 6 h. After the reaction is completed, a natural silk nanofiber grafted ε-polylysine suspension is obtained.

[0087] (3) Preparation of natural silk nanofiber grafted ε-polylysine sponge material: Place the natural silk nanofiber grafted ε-polylysine suspension prepared in step (2) in a refrigerator at -40°C for 12 hours, and then freeze-dry in a freeze dryer at -45°C for 24 hours to obtain a natural silk nanofiber grafted ε-polylysine sponge material.

[0088] Example 3

[0089] This example prepares a natural nanofiber grafted polylysine - natural silk nanofiber grafted α-polylysine sponge material. The reaction mechanism is as follows: Figure 2 shown.

[0090] (1) Preparation of silk nanofiber suspension: Weigh 2 g of silk fiber and add it to a frozen sodium hydroxide / urea aqueous solution, wherein the mass ratio of sodium hydroxide to urea is 5:12, the mass ratio of urea to water is 12:83, and the ratio of the mass of natural fiber to the total mass of sodium hydroxide, urea and water is 1:50; stir with a mechanical stirrer for 10 min every 12 h; centrifuge at 9000 rpm for 10 min after 48 h until the pH is <8; then ultrasonically crush with an ultrasonic crusher for 30 min, and centrifuge at 5000 rpm for 8 min to remove the bottom precipitate to obtain an intermediate suspension; freeze-dry the intermediate suspension at -40°C in a freeze dryer for 20 h to obtain freeze-dried silk nanofibers; add the freeze-dried silk nanofibers (10-1000 nm) to deionized water and centrifuge at 5000 rpm for 10 minutes to obtain a silk nanofiber suspension, wherein the concentration of the silk nanofibers is 3 wt%.

[0091] (2) Preparation of a suspension of natural silk nanofiber grafted with α-polylysine: Add 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide in an amount of 150 μL / mL to the silk nanofiber suspension prepared in step (1) to obtain a premixed solution; then add N-hydroxysuccinimide in an amount of 75 μL / mL to the premixed solution, stir at low temperature for 30 min, and obtain a mixed solution; then, add α-polylysine (number average molecular weight less than 5000 Da) accounting for 5% of the mass of the silk nanofiber to the mixed solution, stir at low temperature at 4°C for 25 min, and carry out grafting reaction at 4°C for 4 h. After the reaction is completed, a suspension of natural silk nanofiber grafted with α-polylysine is obtained.

[0092] (3) Preparation of natural silk nanofiber grafted α-polylysine sponge scaffold: freeze-dry the natural silk nanofiber grafted α-polylysine suspension prepared in step (2) at -45°C for 20 hours to obtain a natural silk nanofiber grafted α-polylysine sponge scaffold, which can be used as a biomedical material.

[0093] Example 4

[0094] This embodiment prepares a natural nanofiber grafted with polylysine, namely, natural silk nanofiber grafted with α-polylysine hydrogel.

[0095] (1) Preparation of silk nanofiber suspension: freeze-dried silk nanofibers (30-300 nm) were added to deionized water and centrifuged at 7000 rpm for 10 minutes to prepare a silk nanofiber suspension with a silk nanofiber concentration of 3 wt%.

[0096] (2) preparing a suspension of natural silk nanofiber grafted with ε-polylysine: adding 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide in an amount of 150 μL / mL to the silk nanofiber suspension prepared in step (1) to obtain a premixed solution; then adding N-hydroxysuccinimide in an amount of 75 μL / mL to the premixed solution, stirring at low temperature for 30 min to obtain a mixed solution; subsequently, adding α-polylysine (number average molecular weight less than 5000 Da) accounting for 5% of the mass of the silk nanofiber to the mixed solution, stirring at low temperature for 40 min at 0°C, and performing a grafting reaction at 0°C for 8 h. After the reaction is completed, a suspension of natural silk nanofiber grafted with α-polylysine is obtained.

[0097] (3) Preparation of natural silk nanofiber grafted α-polylysine hydrogel: Add genipin to the natural silk nanofiber grafted α-polylysine suspension prepared in step (2), wherein the volume ratio of the natural nanofiber grafted polylysine suspension to genipin is 10:5, stir evenly and pour into a mold, place it at room temperature and let it stand to form a gel, thereby obtaining the natural silk nanofiber grafted α-polylysine hydrogel.

[0098] The natural nanofiber suspension and the natural nanofiber grafted polylysine suspension prepared in Example 1 and Example 2 were tested for Tyndall effect. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that the natural nanofiber suspension and the natural nanofiber grafted polylysine suspension prepared in the present invention produce the Tyndall effect, proving that they are suspension systems.

[0099] The Zeta potential test was performed on the natural nanofiber suspension, natural nanofiber grafted polylysine suspension and polylysine solution prepared in Example 1 and Example 2. The results are as follows: Figure 4 As shown. Figure 4 It can be seen that the Zeta potential of natural nanofibers is -44.54 mV, indicating that the amino electrostatic effect on the chain of natural nanofibers is strong, the colloidal dispersion is stable, and it is not easy to agglomerate; polylysine is positively charged. With the introduction of polylysine, the Zeta potential of the nanofibers gradually increases, showing a positive potential, indicating that the natural nanofibers are successfully grafted with polylysine.

[0100] The natural nanofibers and natural nanofiber grafted polylysine prepared in Example 1 and Example 2 were subjected to SEM testing, and the results were as follows: Figure 5 As shown. Figure 5 It can be seen that the size of the natural nanofibers prepared by the alkali, urea and water system of the present invention is at the nanometer level, and the size of the natural nanofibers after grafting polylysine increases slightly, but is still nanometer-sized.

[0101] The natural nanofibers and natural nanofiber grafted polylysine prepared in Example 1 and Example 2 were tested for antibacterial properties. The results are as follows: Figure 6 As shown. Figure 6 It can be seen that natural nanofibers grafted with poly-lysine have good inhibitory effects on Staphylococcus aureus and Escherichia coli.

[0102] The natural nanofibers and natural nanofiber grafted polylysine prepared in Example 1 and Example 2 were tested for food preservation. The results are as follows: Figure 7 As shown. Figure 7 It can be seen that natural nanofibers grafted with polylysine have a better preservation effect.

[0103] It can be seen from the above examples that the natural nanofiber grafted polylysine provided by the present invention has good antibacterial properties and biocompatibility, and has good application prospects in the fields of food preservation and biomedicine.

[0104] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. The present invention provides a natural nanofiber grafted with polylysine, comprising natural nanofiber and polylysine connected to the natural nanofiber via an amide bond.

2. The natural nanofiber grafted polylysine according to claim 1, characterized in that: The natural nanofiber grafted polylysine is natural nanofiber grafted ε-polylysine or natural nanofiber grafted α-polylysine.

3. The natural nanofiber grafted polylysine according to claim 1 or 2, characterized in that: The number average molecular weight of the natural nanofiber grafted with polylysine is 20-500 KDa.

4. The method for preparing the natural nanofiber grafted with polylysine according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) mixing natural fibers, alkali, urea and water to obtain a natural nanofiber suspension; (2) mixing the natural nanofiber suspension with a crosslinking agent and polylysine to carry out a grafting reaction to obtain a natural nanofiber grafted polylysine suspension; The mass ratio of natural nanofibers to polylysine in the natural nanofiber suspension is not less than 5:1; The molar ratio of the carboxyl group of the natural nanofiber to the crosslinking agent in the natural nanofiber suspension is 1:0.1-1.

0.

5. The preparation method according to claim 4, characterized in that: The polylysine includes one or more of ε-polylysine and α-polylysine; the number average molecular weight of the polylysine is less than 5000Da.

6. The preparation method according to claim 4 or 5, characterized in that: The temperature of the grafting reaction is -15 to 10° C., and the insulation time is 2 to 8 hours.

7. Use of the natural nanofiber grafted polylysine as claimed in any one of claims 1 to 3 or the natural nanofiber grafted polylysine obtained by the preparation method according to any one of claims 4 to 6 as an antibacterial material.

8. A method for preparing a natural nanofiber grafted polylysine biofilm, characterized in that: The following steps are involved: drying the natural nanofiber grafted polylysine suspension into a film to obtain a natural nanofiber grafted polylysine biofilm; The natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method according to any one of claims 4 to 6.

9. A method for preparing a natural nanofiber grafted polylysine hydrogel, characterized in that: The following steps are involved: The suspension of natural nanofiber grafted polylysine is mixed with a cross-linking agent and then allowed to stand to form a gel, thereby obtaining a natural nanofiber grafted polylysine hydrogel; The natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method according to any one of claims 4 to 6.

10. A method for preparing a natural nanofiber grafted polylysine sponge material, characterized in that: The following steps are involved: freeze-drying the natural nanofiber grafted polylysine suspension to obtain a natural nanofiber grafted polylysine sponge material; The natural nanofiber grafted polylysine suspension is a natural nanofiber grafted polylysine suspension obtained by the preparation method according to any one of claims 4 to 6.

Citation Information

Patent Citations

  • Method for preparing sericin film by laccase-TEMPO (2,2,6,6-tetramethylpiperidyl-N-oxide) process

    CN105885073A

  • Preparation method of regenerated silk fibroin / epsilon-polylysine composite hydrogel as well as product and application of regenerated silk fibroin / epsilon-polylysine composite hydrogel

    CN114835917A

  • Natural silk nano fibril with antibacterial property as well as preparation method and application of natural silk nano fibril

    CN116949817A

  • UHMWPE (Ultra High Molecular Weight Polyethylene) composite fiber with functional coating and preparation method thereof

    CN117090047A

  • Antimicrobial blend mass and its production

    JP1999049620A