Cotton foam real leather feeling PU leather and preparation method thereof
By adopting specific glue and surface formulas and processing methods in the PU leather, the problems of hard feel and poor cotton bubble feel in traditional PU leather are solved, and a softer and plumper cotton bubble leather feel is achieved, which improves the interior of the car The quality and user experience of decoration.
Patent Information
- Application Number
- CN202411416332.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional PU leather has a hard feel, poor plumpness and cotton bubble feel, and cannot provide a similar user experience as natural leather.
Cotton foam leather with four-layer superposition structure includes base cloth, glue layer, surface layer and surface treatment layer. The glue layer is distributed by component A and group B. Component A contains polybutylene glycol and foaming agent , methyl ethyl ketone and flame retardant, component B is toluene diisocyanate, the surface layer consists of polyurethane resin, N,N-dimethylformamide and methylethyl ketone, and the surface treatment layer is made of dipropylene glycol Dimethyl ether and ethanol are prepared in a mixing manner, and are uniformly scraped and dried by specific processing conditions and equipment.
It improves the compactness and softness of the PU leather, enhances elasticity and fullness, and enhances the sense of luxury and user experience of the car interior.
Smart Images

Figure CN119083198A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to leather materials, and in particular relates to a cotton foam genuine leather feeling PU leather and a preparation method thereof. Background Art
[0002] PU leather, also known as synthetic or artificial leather, has the advantages of durability, waterproofness, easy cleaning, and good processing performance. It is an ideal imitation leather product to replace natural leather. At present, PU leather is widely used in clothing, shoes, bags, furniture and other industries. Figure 1 As shown, traditional PU leather is often a four-layer stacked structure, from bottom to top, it is base fabric, adhesive layer, surface layer, and surface treatment layer. However, traditional PU leather does not have the feel of cotton-foam leather. It feels hard, and has poor fullness and cotton-foam feel. The reason for this is related to the previous PU leather processing materials and processes.
[0003] In order to solve the above problems existing in the prior art, the present invention is provided. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention provides a PU leather with a cotton-foam feel and a preparation method thereof, which solves the problems of the traditional PU leather having a hard feel and poor fullness and cotton-foam feel.
[0005] The technical solution of the present invention is:
[0006] A cotton foam genuine leather PU leather, the cotton foam genuine leather PU leather comprising a base fabric, a glue layer, a surface layer and a surface treatment layer arranged in sequence from bottom to top;
[0007] The adhesive layer is made of an adhesive layer liquid prepared from component A and component B. Calculated by weight, the component A includes 80-100 parts of polybutylene glycol, 0.5-4 parts of foaming agent, 5-10 parts of methyl ethyl ketone, and 30-50 parts of flame retardant; the component B is 80-100 parts of toluene diisocyanate; and the mass ratio of the component B to the component A is 0.65±0.05:1.
[0008] Preferably, the foaming agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and the foaming temperature thereof is controlled at 100-140°C; and the flame retardant is aluminum hypophosphite.
[0009] Preferably, the surface layer is prepared from the following components in parts by mass: 80-100 parts of polyurethane resin, 20-25 parts of N,N-dimethylformamide, 20-25 parts of methyl ethyl ketone, and 20-25 parts of isopropanol.
[0010] Preferably, the surface treatment layer is prepared from the following components in parts by mass: 70-100 parts of dipropylene glycol dimethyl ether, 5-10 parts of ethanol, and 10-120 parts of octamethylcyclotetrasiloxane.
[0011] Preferably, the base fabric of the cotton foam genuine leather PU leather is a weft-knitted 3D Mesh lining, the lining width is controlled at 1570mm-1630mm, the lining density is controlled at warp density [cpi] 40±2, weft density [wpi] 40±2, and the lining thickness is controlled at 2.5-3.5mm. The lining is thick and soft to the touch.
[0012] A method for preparing cotton foam genuine leather PU leather comprises the following steps:
[0013] S1. Apply the mixed surface liquid evenly on the release paper through a linked scraper, and dry it in an oven. The processing conditions are temperature: 120℃-140℃, processing speed: 10m / min, and the gram weight is controlled at 30-45g / m 2 ;
[0014] S2. Then mix the A / B components in proportion with a glue mixer and apply them on the surface. The temperature is controlled at 100℃-140℃ and the weight is controlled at 150-300g / m 2 ;
[0015] S3, when the adhesive layer is semi-dry, attach the base fabric, and dry it at 120℃-140℃;
[0016] S4, separating the PU leather semi-finished product with the surface layer, the adhesive layer and the base fabric from the release paper to form a PU leather embryo leather;
[0017] S5. Use roller coating equipment to roll the surface treatment liquid on the PU leather embryo, the drying temperature is 120℃-140℃, the processing speed is 10m / min, and the gram weight is controlled at 7-12g / m 2 , and finally the cotton foam genuine leather PU leather is produced.
[0018] Preferably, the preparation method of component A is as follows: polybutylene glycol, foaming agent, methyl ethyl ketone and flame retardant are mixed according to the proportion, stirred for 10±2 hours, the viscosity is controlled at 6000-9000cps, and sealed for standby use; component B is toluene diisocyanate.
[0019] Preferably, polyurethane resin, N,N-dimethylformamide, methyl ethyl ketone and isopropyl alcohol are mixed according to a ratio, stirred for 4±1 hr, and the viscosity is controlled at 2000-3000 cps to obtain a surface layer liquid.
[0020] Preferably, dimethyl ether of dipropylene glycol, ethanol and octamethylcyclotetrasiloxane are mixed according to a ratio, stirred for 4±1 hr, and the viscosity is controlled at 100-1000 cps to obtain a surface treatment liquid.
[0021] The beneficial effects of the present invention are:
[0022] The foaming agent used in the glue layer of the present invention is 4,4'-oxybisbenzenesulfonyl hydrazide, which has a simple use method and low requirements. The PU leather processed by the present invention has low density, soft hand feel, high elasticity and high fullness, which helps to improve the high-grade sense of automobile interior and enhance people's use experience. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0024] Figure 1 This is a schematic diagram of the traditional PU leather structure;
[0025] Figure 2 It is a schematic diagram of the structure of the cotton foam genuine leather feeling PU leather of the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0027] like Figure 2 As shown, the cotton foam genuine leather PU leather prepared in the following embodiments also has a four-layer stacked structure, which includes a base fabric, an adhesive layer, a surface layer, and a surface treatment layer from bottom to top.
[0028] The material names corresponding to each English abbreviation are as follows:
[0029] PTMG: polytetramethylene glycol, specifically PTMG2000; MEK: methyl ethyl ketone; TDI: toluene diisocyanate, specifically 2,6-TDI; DMF: N,N-dimethylformamide; IPA: isopropyl alcohol.
[0030] Example 1
[0031] The raw materials used in each layer are as follows, and each number is by mass:
[0032] Base fabric: The base fabric is made of weft-knitted 3D Mesh lining, the lining width should be controlled at 1570mm-1630mm, the lining density should be controlled at warp density [cpi] 40±2 and weft density [wpi] 40±2, 3Dmesh, the lining thickness is controlled at 2.5-3.5mm, the lining is thick and soft to the touch.
[0033] Adhesive layer formula: composed of component A and component B;
[0034] A component formula: PTMG 85 parts, foaming agent 4,4'-oxybisbenzenesulfonyl hydrazide 2.5 parts, MEK 5 parts, aluminum hypophosphite 35 parts, after fully stirring and mixing the above materials for 10 hours, the viscosity is controlled at 6000-9000cps, and it can be used. The foaming agent used in the A component formula is 4,4'-oxybisbenzenesulfonyl hydrazide, and its characteristic foaming temperature should be controlled at 100-140℃.
[0035] Formula of component B: 85 parts of TDI.
[0036] Surface layer formula: 85 parts of polyurethane resin, 22 parts of DMF, 22 parts of MEK, 22 parts of IPA. After stirring and mixing for 4 hours, the viscosity can be controlled at 2000-3000cps and can be used.
[0037] The surface treatment layer formula is: 85 parts of dipropylene glycol dimethyl ether, 7 parts of ethanol, and 60 parts of octamethylcyclotetrasiloxane. After stirring and mixing for 4 hours, the viscosity is controlled to 100-1000cps and can be used.
[0038] The preparation method of the cotton foam genuine leather PU leather of the present embodiment is as follows:
[0039] 1. Prepare the surface liquid according to the surface formula, and evenly apply the mixed surface liquid on the release paper through a linked scraper, and dry it in an oven. The processing conditions are temperature: 120℃; processing speed: 10m / min; control the gram weight at 40g / m 2 .
[0040] 2. According to the glue layer formula, the A component formula and the B component formula are mixed to obtain the glue layer liquid, and then the glue layer liquid is scraped on the surface layer, and the temperature is controlled at 105℃; the gram weight is controlled at 200g / m 2 .
[0041] 3. When the adhesive layer is semi-dry, laminate the 3DMesh base fabric with a laminating pressure of about 3kg and a drying temperature of 120℃.
[0042] 4. Separate the PU leather semi-finished product with the surface layer, adhesive layer and base fabric from the release paper to form PU leather embryo leather.
[0043] 5. Prepare the surface treatment liquid according to the surface treatment layer formula, and use roller coating equipment to roll the surface treatment liquid on the PU leather embryo. The drying temperature is 125℃, the processing speed is 10m / min, and the gram weight is 8g / m 2 .
[0044] Finally, the foamed genuine leather PU leather was obtained.
[0045] Example 2
[0046] Compared with Example 1, the difference of this embodiment lies in the formula of the adhesive layer. The formula of the adhesive layer of this embodiment is as follows:
[0047] A component formula: PTMG 95 parts, foaming agent 4,4'-oxybisbenzenesulfonyl hydrazide 3 parts, MEK 7 parts, aluminum hypophosphite 45 parts, after fully stirring and mixing the above materials for 10 hours, the viscosity is controlled at 6000-9000cps, and it can be used. The foaming agent used in the A component formula is 4,4'-oxybisbenzenesulfonyl hydrazide, which has the characteristics of controlling the foaming temperature at 100-140℃, the foaming particle size is less than 50 microns, and it cannot be used together with DMF.
[0048] Formula of component B: 95 parts of TDI.
[0049] Example 3
[0050] The difference between this embodiment and embodiment 1 is only in the preparation method. The preparation method of this application is as follows:
[0051] 1. Prepare the surface liquid according to the surface formula, and evenly apply the mixed surface liquid on the release paper through a linked scraper, and dry it in an oven. The processing conditions are temperature: 135℃; processing speed: 10m / min; control the gram weight at 40g / m 2 .
[0052] 2. According to the glue layer formula, the A component formula is mixed with the B component formula to obtain the glue layer liquid, and then the glue layer liquid is scraped on the surface layer, and the temperature is controlled at 105℃; the gram weight is controlled at 180g / m 2 .
[0053] 3. When the adhesive layer is semi-dry, laminate the 3DMesh base fabric with a laminating pressure of about 3kg and a drying temperature of 130℃.
[0054] 4. Separate the PU leather semi-finished product with the surface layer, adhesive layer and base fabric from the release paper to form PU leather embryo leather.
[0055] 5. Prepare the surface treatment liquid according to the surface treatment layer formula, and use roller coating equipment to roll the surface treatment liquid on the PU leather embryo. The drying temperature is 130℃, the processing speed is 10m / min, and the gram weight is 10g / m 2 .
[0056] Comparative Example 1
[0057] The number of processing layers in this comparative example is the same as that in the embodiment; the raw materials used in each layer are as follows, and each number is by mass:
[0058] Base fabric: The base fabric is made of weft-knitted 3D Mesh lining, the lining width should be controlled at 1570mm-1630mm, the lining density should be controlled at warp density [cpi] 40±2 and weft density [wpi] 40±2, 3Dmesh, the lining thickness is controlled at 2.5-3.5mm, the lining is thick and soft to the touch.
[0059] Adhesive layer formula: composed of component A and component B;
[0060] Formula of component A: 85 parts of PTMG, 5 parts of MEK, and 35 parts of aluminum hypophosphite. After the above materials are fully stirred and mixed for 10 hours, the viscosity is controlled at 6000-9000cps.
[0061] Formula of component B: 85 parts of TDI.
[0062] Surface layer formula: 85 parts of polyurethane resin, 22 parts of DMF, 22 parts of MEK, 22 parts of IPA. After stirring and mixing for 4 hours, the viscosity can be controlled at 2000-3000cps and can be used.
[0063] The surface treatment layer formula is: 85 parts of dipropylene glycol dimethyl ether, 7 parts of ethanol, and 60 parts of octamethylcyclotetrasiloxane. After stirring and mixing for 4 hours, the viscosity is controlled to 100-1000cps and can be used.
[0064] The preparation method of the cotton foam genuine leather PU leather of this comparative example is as follows:
[0065] 1. Prepare the surface liquid according to the surface formula, and evenly apply the mixed surface liquid on the release paper through a linked scraper, and dry it in an oven. The processing conditions are temperature: 120℃; processing speed: 10m / min; control the gram weight at 40g / m 2 .
[0066] 2. According to the glue layer formula, the A component formula and the B component formula are mixed to obtain the glue layer liquid, and then the glue layer liquid is scraped on the surface layer, and the temperature is controlled at 90℃; the gram weight is controlled at 200g / m 2 .
[0067] 3. When the adhesive layer is semi-dry, laminate the 3DMesh base fabric with a laminating pressure of about 3kg and a drying temperature of 130℃.
[0068] 4. Separate the PU leather semi-finished product with the surface layer, adhesive layer and base fabric from the release paper to form PU leather embryo leather.
[0069] 5. Prepare the surface treatment liquid according to the surface treatment layer formula, and use roller coating equipment to roll the surface treatment liquid on the PU leather embryo. The drying temperature is 125℃, the processing speed is 10m / min, and the gram weight is 8g / m 2 .
[0070] Finally, the foamed genuine leather PU leather was obtained.
[0071] The BLC values of the PU leathers of the embodiments and comparative examples are shown in Table 1. The smaller the BLC value, the harder the leather, and the larger the BLC value, the softer the leather.
[0072] Table 1 BLC values of PU leather in various embodiments and comparative examples
[0073]
[0074] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A cotton foam genuine leather PU leather, characterized in that: The PU leather with cotton foam genuine leather feeling comprises a base fabric, a glue layer, a surface layer and a surface treatment layer arranged in sequence from bottom to top; The adhesive layer is made of an adhesive layer liquid prepared from component A and component B. Calculated by weight, the component A includes 80-100 parts of polybutylene glycol, 0.5-4 parts of foaming agent, 5-10 parts of methyl ethyl ketone, and 30-50 parts of flame retardant; the component B is 80-100 parts of toluene diisocyanate; and the mass ratio of the component B to the component A is 0.65±0.05:
1.
2. The cotton foam genuine leather PU leather according to claim 1, characterized in that: The foaming agent is 4,4'-oxybisbenzenesulfonyl hydrazide, and its foaming temperature is controlled at 100-140°C; the flame retardant is aluminum hypophosphite.
3. The cotton foam genuine leather PU leather according to claim 1, characterized in that: The surface layer is prepared from the following components in parts by mass: 80-100 parts of polyurethane resin, 20-25 parts of N,N-dimethylformamide, 20-25 parts of methyl ethyl ketone, and 20-25 parts of isopropanol.
4. The cotton foam genuine leather PU leather according to claim 1, characterized in that: The surface treatment layer is prepared from the following components in parts by mass: 70-100 parts of dipropylene glycol dimethyl ether, 5-10 parts of ethanol, and 10-120 parts of octamethylcyclotetrasiloxane.
5. A method for preparing the cotton foam genuine leather PU leather according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Apply the mixed surface liquid evenly on the release paper through a linked scraper, and dry it in an oven. The processing conditions are temperature: 120℃-140℃, processing speed: 10m / min, and the gram weight is controlled at 30-45g / m 2 ; S2. Then use a glue mixer to mix components A and B and apply them on the surface. The temperature is controlled at 100℃-140℃ and the weight is controlled at 150-300g / m 2 ; S3, when the adhesive layer is semi-dry, attach the base fabric, and dry it at 120℃-140℃; S4, separating the PU leather semi-finished product with the surface layer, the adhesive layer and the base fabric from the release paper to form a PU leather embryo leather; S5. Use roller coating equipment to roll the surface treatment liquid on the PU leather embryo, the drying temperature is 120℃-140℃, the processing speed is 10m / min, and the gram weight is controlled at 7-12g / m 2 , and finally the cotton foam genuine leather PU leather is produced.
6. The preparation method according to claim 5, characterized in that The preparation method of component A is as follows: polybutylene glycol, foaming agent, methyl ethyl ketone and flame retardant are mixed according to the proportion, fully stirred for 10±2 hours, the viscosity is controlled at 6000-9000cps, and sealed for use; component B is toluene diisocyanate.
7. The preparation method according to claim 5, characterized in that According to the ratio, polyurethane resin, N,N-dimethylformamide, methyl ethyl ketone and isopropyl alcohol are mixed and stirred for 4±1 hours, and the viscosity is controlled at 2000-3000 cps to obtain a surface layer liquid.
8. The preparation method according to claim 5, characterized in that According to the ratio, dimethyl ether of dipropylene glycol, ethanol and octamethylcyclotetrasiloxane are mixed, stirred for 4±1 hr, and the viscosity is controlled at 100-1000 cps to obtain a surface treatment liquid.
Citation Information
Patent Citations
Low energy consumption ecological leatheroid preparation method
CN103669021A
Composite leather and manufacturing method thereof
CN108505350A
Synthetic leather and preparation method thereof
CN116065405A
High-performance microsphere foaming agent
CN116903922A
Synthetic leather capable of being rapidly cooled and preparation method thereof
CN118621599A