Textile with irregular photonic crystal texture patterns and preparation method thereof

By applying charge effect modifier and nano-microsphere printing slurry to the textiles, irregular photonic crystal texture patterns are formed, which solves the problems of pattern repeatability and complex process in the industrial production of textiles, and realizes textile production with unique texture and iridescent effects , suitable for large-scale industrial applications.

CN119083209AActive Publication Date: 2024-12-06ZHEJIANG SCI-TECH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411209697.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The prior art is difficult to industrially produce irregular photonic crystal texture patterns on textiles, resulting in pattern repeatability and complex process, which cannot meet the needs of personalization and uniqueness.

Method used

By applying a charge effect modifier on the surface of the fabric, combined with the nano-microsphere printing slurry, the principles of homogeneous charge repulsion and heterogeneous charge suction are used to promote local enrichment and supersaturation of charged colloidal nano-microspheres, forming irregularities photonic crystal texture pattern.

Benefits of technology

It realizes the rapid and simple large-area preparation of irregular photonic crystal texture patterns on textiles, with unique texture and iridescent effects, suitable for industrial production, and the pattern of each product is unique.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083209A_ABST
    Figure CN119083209A_ABST
Patent Text Reader

Abstract

The invention relates to the field of textile structure color generation, in particular to a textile with irregular photonic crystal texture patterns and a preparation method of the textile. The method comprises the following steps: S1, uniformly mixing a nano-microsphere dispersion liquid, a high-boiling-point additive, a stray light absorbent and a surfactant to obtain nano-microsphere printing paste; s2, applying an aqueous solution of a charge effect modifier to the surface of the hydrophobic fabric, and performing subsequent heating drying / non-heating drying treatment according to the performance of the charge effect modifier and an application method to obtain a modified fabric; s3, applying nano-microsphere printing paste to the surface of the modified fabric obtained in S2; and S4, heating and assembling the modified fabric containing the nano-microsphere coating obtained in the step S3 to obtain the textile with the irregular photonic crystal texture pattern. According to the method, the charge effect is utilized, the photonic crystal structure color generation pattern with the iridescent effect and high structural stability can be simply, conveniently and rapidly generated on the fabric, the textile is endowed with unique attractiveness and fashionability, and the method is suitable for large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of textile structural coloration, and in particular to a textile with an irregular photonic crystal texture pattern and a preparation method thereof. Background Art

[0002] Photonic crystals are a type of crystalline material formed by two or more substances with different dielectric constants (refractive index) arranged in a certain periodic space. This special periodic structure gives it unique optical controllability, and is therefore widely used in display devices, detection, sensing, anti-counterfeiting marks, fashion textiles and other fields. Patterned coloring of textiles is an important means to increase the added value of textile products and meet personalized aesthetic needs. Patterned photonic crystals with iridescent effects not only have specific pattern effects, but also present high brightness, high saturation and smart structural color visual effects, which have great development prospects in the fields of ecological textiles, fashion textiles and smart textiles.

[0003] At present, the preparation technologies of patterned photonic crystals include optical etching technology, mask technology, inkjet printing technology, screen printing technology, etc. Among them, although optical etching technology is relatively mature, it requires expensive and sophisticated equipment and is difficult to be widely used; mask technology is difficult to achieve industrial production due to template limitations; inkjet printing technology is hindered from industrial application due to easy clogging of the nozzle; screen printing is currently the most commonly used method for constructing patterned photonic crystals. Zhou et al. (Zhou C, Qi Y, Zhang S, et al. Rapid fabrication of vivid noniridescent structural colors on fabrics with robust structural stability by screen printing [J]. Dyes and Pigments, 2020, 176: 108-226.) prepared a printing paste with polyacrylate (PA) water-based adhesive, carbon black and polystyrene microspheres, and printed it on white polyester fabric by screen printing to obtain a non-iridescent color pattern. Due to the bonding effect of PA, the prepared photonic crystal has strong structural stability and the outline of the structural color pattern is clearer, but because the PA macromolecules (accounting for 8wt% of the nanospheres) in the printing paste greatly affect the regular assembly of the nanospheres, the printed pattern effect is similar to the wide viewing angle of the dye, the saturation and brightness of the structural color are low, and the unique iridescence effect of the photonic crystal structural color is lost. Chinese patent document CN115233473A prints a photonic crystal structure color pattern with a scintillation effect on fabrics by screen printing. This method adds a synthetic thickener with high thickening ability to the printing paste to play a viscosity regulating role, which is conducive to obtaining a clear outline of the group pattern, but the addition of the thickener is bound to affect the assembly of the nanospheres to a certain extent, so that a short-range ordered-long-range quasi-ordered photonic crystal pattern is obtained, which has a certain scintillation effect but no obvious iridescence effect. Chinese patent document CN115287919A constructs a hydrophilic-hydrophobic difference pattern on the surface of a textile substrate by screen printing, and combines shear-induced assembly to confine the assembly of liquid photonic crystals in the hydrophilic pattern area. The prepared patterned photonic crystals have both good contour clarity and significant iridescence effect. Although this method can obtain a photonic crystal pattern with an iridescence effect, the process is complicated. Moreover, due to the limitation of the pattern, the pattern of the industrial product of the screen printing method is repetitive.With the improvement of people's living standards, people have higher and higher requirements for the aesthetics of textiles. The pursuit of individuality and uniqueness has become a fashion trend. Textiles with irregular texture patterns are favored by people. For example, the Chinese folk batik art produces a natural ice effect that is difficult to imitate artificially, making each product unique and showing a fresh and natural beauty. However, it is still a difficult problem to achieve the industrial production of textiles with irregular photonic crystal texture patterns through the currently commonly used printing technology. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing textiles with irregular photonic crystal texture patterns. The method utilizes the charge effect to simply and quickly produce photonic crystal structure color-producing patterns with iridescent effects and high structural stability on the fabric, giving the textiles unique aesthetics and fashion, and is suitable for large-scale industrial applications.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] A method for preparing a textile having an irregular photonic crystal texture pattern, the method comprising the following steps:

[0007] S1. Preparation of nano-microsphere printing paste

[0008] The nanosphere dispersion, high boiling point additive, stray light absorber and surfactant are uniformly mixed to obtain the nanosphere printing paste; wherein the solid content of the nanosphere dispersion is 25% to 55%. Based on the weight of the nanosphere dispersion as 100%, the amount of the high boiling point additive is 0.5 to 6% of the weight of the nanosphere dispersion, the amount of the stray light absorber is 0 to 0.3% of the weight of the nanosphere dispersion, and the amount of the surfactant is 2 to 8% of the weight of the nanosphere dispersion;

[0009] The high boiling point additive is selected from one or a mixture of glycerol, propylene glycol, formamide, and ethylene glycol;

[0010] The surfactant is selected from one or a mixture of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene sorbitan fatty acid ester, fatty acid methyl ester ethoxylate or ethylene oxide adduct of polypropylene glycol;

[0011] The stray light absorber is selected from one or a mixture of black dye, nano carbon black or water-soluble black pigment;

[0012] S2, applying an aqueous solution of a charge effect modifier on the surface of a hydrophobic fabric, and performing subsequent heating and drying / non-heating and drying treatment according to the performance and application method of the charge effect modifier to obtain a modified fabric;

[0013] The charge effect modifier is an ionic surfactant or a charged polymer. When the charge effect modifier is an ionic surfactant, the concentration is 0.1 to 30 wt %; when the charge effect modifier is a charged polymer, the concentration is 0.01 to 0.8 wt %;

[0014] S3, applying nano-microsphere printing paste on the surface of the modified fabric obtained in S2;

[0015] S4. The modified fabric containing the nano-microsphere coating obtained in S3 is heated and assembled to obtain a textile having an irregular photonic crystal texture pattern.

[0016] In S2 of the present invention, if the nano-microsphere printing paste applied subsequently adopts hard-core-soft-shell nano-microspheres, the above-mentioned modifier can be directly applied to the surface of the tightly structured hydrophobic fabric; for hydrophilic or loosely structured fabrics, water-repellent finishing or coating finishing is required. If the nano-microsphere printing paste applied subsequently adopts hard nano-microspheres, in order to improve the stability of the assembly structure, before applying the charge effect modifier, it is necessary to construct an appropriate polymer film on the fabric surface according to the Chinese invention patent "Large-area preparation method of high-stability and high-saturation photonic crystal structure color-forming fabric" (ZL202111437620.8), that is, the fabric with a polymer layer obtained by heating and curing the special polymer described in the patent to form a film.

[0017] The preparation method of the present invention can form an irregular photonic crystal pattern on a textile substrate to obtain a textile having both a unique texture pattern effect and a photonic crystal iridescent effect structural color, thereby achieving the beauty and uniqueness of the pattern and color.

[0018] Preferably, the nanoparticles described in S1 are colloidal nanoparticles with ionic groups or negatively or positively charged surfaces, including

[0019] Organic polymer colloidal nanospheres: polystyrene (PS), polymethyl methacrylate (PMMA), polystyrene@polyacrylic acid (PS@PAA), polystyrene@polydopamine (PS@PDA), poly(styrene-hydroxyethyl acrylate) (P(St-HEA)), poly(styrene-methyl methacrylate) (P(St-MMA)), poly(styrene-methacrylic acid) (P(St-MAA)), polystyrene@poly(methyl methacrylate-butyl acrylate) (PS@P(MMA-BA)), polymethyl methacrylate@poly(hydroxyethyl acrylate-hydroxyethyl methacrylate) (PMAA@P(HEA-HEMA)), poly(styrene-methacrylic acid)@poly(ethyl acrylate-methacrylic acid) (P(St-MAA)@P(EA-MAA)) nanospheres,

[0020] Inorganic colloidal nanoparticles of silica (SiO2), titanium dioxide (TiO2), zirconium oxide (ZrO) nanoparticles, or

[0021] Any one of organic@inorganic and inorganic@organic colloidal nanospheres, polystyrene@silica (PS@SiO2) and silica@polystyrene (SiO2@PS) nanospheres.

[0022] Preferably, the ionic surfactants in S2 include anionic surfactants and cationic surfactants, the anionic surfactants include sodium stearate, sodium palmitate, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate; the cationic surfactants include hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide or hexadecylpyridinium chloride; the charged natural or synthetic polymers include sodium alginate, carboxymethyl cellulose, sodium polyacrylate and their derivatives.

[0023] Preferably, the charge effect modifier in S2 is applied by dipping, padding or coating.

[0024] Preferably, the subsequent heating and drying / non-heating drying treatment is carried out according to the performance and application method of the charge effect modifier as described in S2, specifically: when an ionic surfactant is used, the modified fabric needs to be heated and dried, the drying temperature is 60-90°C, and the drying time is 2-5 minutes; when a charged polymer is used, the liquid carrying rate of the modified fabric is controlled to be 5-80% without heating and drying treatment, and the next step of processing is directly carried out.

[0025] Preferably, the hydrophobic fabric described in S2 has a water contact angle of 110° to 180°.

[0026] Preferably, the nano-microsphere printing paste described in S3 is applied by blade coating or spraying.

[0027] Preferably, in the heating assembly described in S4, the assembly temperature is 40 to 130° C. and the assembly time is 3 to 60 minutes.

[0028] Preferably, the fabric is selected from polyester fabric, nylon fabric, cotton fabric, silk fabric, polyester-cotton blended fabric or polyester-spandex blended fabric.

[0029] A textile with irregular photonic crystal texture pattern prepared according to the preparation method of the present invention.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The present invention applies a charge effect modifier on the surface of the fabric and utilizes the basic physical principle that like charges repel each other and opposite charges attract each other, so as to promote the local enrichment and supersaturation crystallization of charged colloidal nano-microspheres on the textile substrate modified by the charge effect modifier, thereby forming an irregular photonic crystal texture pattern, thereby obtaining a textile with both a unique texture pattern and an iridescent effect structural color, so that the pattern of each textile product is unique;

[0032] 2. The size of the light and dark areas of the irregular pattern prepared by the present invention can be adjusted, and the modifier that can produce the charge effect is widely available, inexpensive, environmentally friendly, requires a small amount, and is easy to use;

[0033] 3. The method of the present invention for preparing irregularly patterned photonic crystal textiles is simple and efficient, can be prepared quickly over a large area, and is suitable for continuous industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 1;

[0035] Figure 2 is a digital photo of the textile with irregular photonic crystal texture pattern prepared in Example 2 (left) and its reflectivity curve (right);

[0036] Figure 3 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 3;

[0037] Figure 4 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 4;

[0038] Figure 5 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 5;

[0039] Figure 6 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 6;

[0040] Figure 7 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 7, wherein a is the sample pattern photographed when the angle between the observation angle and the normal is 0°, and b is the sample pattern photographed when the angle between the observation angle and the normal is 45°;

[0041] Figure 8is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 8, wherein a is a sample pattern taken when the angle between the observation angle and the normal is 0°, b is a sample pattern taken when the angle between the observation angle and the normal is 45°, and c is a sample pattern taken when the angle between the observation angle and the normal is 75°;

[0042] Fig. 9 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 9, wherein a is the sample pattern photographed when the angle between the observation angle and the normal is 0°, and b is the sample pattern photographed when the angle between the observation angle and the normal is 45°;

[0043] Fig.10 is a digital photograph of the textile with irregular photonic crystal texture pattern prepared in Example 10;

[0044] Fig.11 is a digital photograph of a textile without a texture pattern prepared in Comparative Example 1;

[0045] Fig.12 is a digital photograph of a textile without a texture pattern prepared in Comparative Example 2;

[0046] Fig.13 is a digital photo of a textile without a texture pattern prepared in Comparative Example 3, wherein a is a sample pattern photographed on the front side of the fabric, and b is a sample pattern photographed on the back side of the fabric;

[0047] Fig.14 is a digital photograph of a textile without a texture pattern prepared in Comparative Example 4;

[0048] Fig.15 This is a digital photograph of the textile without texture pattern prepared in Comparative Example 5. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further described in detail below through specific embodiments. It should be understood that the implementation of the present invention is not limited to the following embodiments, and any form of modification and / or change made to the present invention will fall within the protection scope of the present invention.

[0050] In the present invention, unless otherwise specified, all parts and percentages are by weight, and the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0051] The reagents used in the following examples, unless otherwise specified, can be purchased from conventional biochemical reagent stores.

[0052] Surfactants and sodium alginate were purchased from Zhejiang Chuanhua Co., Ltd., special polymer ① (PUE1401) from Shanghai Sisheng Polymer Materials Co., Ltd., sodium dodecyl sulfate from Aladdin Reagent (Shanghai) Co., Ltd., and sodium dodecylbenzene sulfonate from Shanghai MacLean Biochemical Technology Co., Ltd. (some of the products are listed, but not limited to the above products).

[0053] The polyester fabric with a special polymer film described in the present invention is a fabric with a polymer layer obtained by heating and curing a special polymer into a film according to the Chinese invention patent "Large-area preparation method of high-stability and high-saturation photonic crystal structure color-producing fabric" (ZL202111437620.8), wherein the special polymer includes a soft-segment and hard-segment copolymerized polyurethane polymer, or a soft-segment and hard-segment copolymerized polyacrylic polymer;

[0054] The specific preparation method of the polyester fabric with special polymer film used in the following examples is: 8 g / m2 of special polymer ① (PUE1401) is scraped on the surface of the polyester fabric and placed in a heating device for heating and curing at 80° C. for 5 minutes to form a film.

[0055] Example 1

[0056] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0057] (1) preparing nanosphere printing paste: a PS@P(MMA-BA) nanosphere dispersion having a particle size of 180 nm and a mass fraction of 45% is mixed with 3% propylene glycol, 0.12% water-soluble black pigment, and 5% polyoxyethylene sorbitan fatty acid ester, based on 100% of the weight of the nanosphere dispersion, and the mixture is set aside;

[0058] (2) coating a 0.5% sodium dodecylbenzene sulfonate aqueous solution on the surface of a white water-repellent finished polyester fabric, and then heating the fabric at 90° C. for 2 min to obtain a fabric modified by a charge effect modifier;

[0059] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric, wherein the thickness of the paste is about 0.1 mm;

[0060] (4) The fabric containing the nano-microspheres was placed in an oven at 130° C. and heated for 15 min to obtain a textile with an irregular photonic crystal texture pattern.

[0061] Example 2

[0062] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0063] (1) Preparation of nano-microsphere printing paste: a PS@P (MMA-BA) nano-microsphere dispersion having a particle size of 190 nm and a mass fraction of 25% is mixed with 0.5% ethylene glycol, 0.24% nano carbon black, and 3% fatty alcohol polyoxyethylene ether, based on 100% by weight of the nano-microsphere dispersion, and the mixture is set aside;

[0064] (2) placing a white water-repellent treated polyester fabric in a 5% sodium dodecyl sulfate aqueous solution for 10 seconds, with a liquid carrying rate of 70%, and heating it at 90° C. for 2 minutes to obtain a fabric modified by a charge effect modifier;

[0065] (3) spraying the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0066] (4) The fabric containing the nano-microspheres is placed in an oven at 120° C. and heated for 20 min to obtain a textile with an irregular photonic crystal texture pattern.

[0067] Example 3

[0068] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0069] (1) preparing nano-microsphere printing paste: uniformly mixing a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 185 nm and a mass fraction of 35%, 1% formamide and 4% polyoxyethylene sorbitan fatty acid ester based on 100% of the weight of the nano-microsphere dispersion, and setting aside;

[0070] (2) coating a 3% sodium dodecyl sulfate aqueous solution on the surface of a black cotton fabric that had been water-repellent finished, and then heating it at 90° C. for 2 min to obtain a fabric modified by a charge effect modifier;

[0071] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0072] (4) The fabric containing the nano-microspheres is placed in an oven at 90° C. and heated for 40 min to obtain a textile with an irregular photonic crystal texture pattern.

[0073] Example 4

[0074] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0075] (1) Preparation of nano-microsphere printing paste: a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 198 nm and a mass fraction of 25% is mixed with 3% propylene glycol and 3% fatty alcohol polyoxyethylene ether based on 100% of the weight of the nano-microsphere dispersion, and the mixture is set aside;

[0076] (2) coating a 4% aqueous solution of hexadecyltrimethylammonium bromide on the surface of a black water-repellent treated silk fabric, and then heating the fabric at 70° C. for 3 min to obtain a fabric modified by a charge effect modifier;

[0077] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0078] (4) The fabric containing the nano-microspheres was placed in an oven at 80° C. and heated for 30 min to obtain a textile with an irregular photonic crystal texture pattern.

[0079] Example 5

[0080] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0081] (1) Preparation of nano-microsphere printing paste: a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 188 nm and a mass fraction of 46% is mixed with 6% propylene glycol and 7% fatty alcohol polyoxyethylene ether based on 100% of the weight of the nano-microsphere dispersion, and the mixture is set aside;

[0082] (2) coating a 0.2% sodium alginate aqueous solution on the surface of a black water-repellent finished polyester-cotton blended fabric to obtain a fabric modified by a charge effect modifier;

[0083] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0084] (4) The fabric containing the nano-microspheres was placed in an oven at 110° C. and heated for 25 min to obtain a textile with an irregular photonic crystal texture pattern.

[0085] Example 6

[0086] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0087] (1) preparing nano-microsphere printing paste: a PS@P(MMA-EA) nano-microsphere dispersion having a particle size of 256 nm and a mass fraction of 45% is mixed with 5% propylene glycol, 0.22% water-soluble black pigment, and 6% fatty acid polyoxyethylene ester, based on 100% of the weight of the nano-microsphere dispersion, and the mixture is set aside;

[0088] (2) coating a 0.4% sodium polyacrylate aqueous solution on the surface of a white cotton fabric that has been water-repellent finished to obtain a fabric modified by a charge effect modifier;

[0089] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0090] (4) The fabric containing the nano-microspheres is placed in an oven at 90° C. and heated for 30 min to obtain a textile with an irregular photonic crystal texture pattern.

[0091] Example 7

[0092] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0093] (1) Preparation of nano-microsphere printing paste: a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 255 nm and a mass fraction of 35% is mixed with 1% propylene glycol, 0.20% nano carbon black, and 4% fatty alcohol polyoxyethylene ether, based on the weight of the nano-microsphere dispersion being 100%, and the mixture is set aside;

[0094] (2) coating a 6% sodium dodecyl sulfate aqueous solution on the surface of a white water-repellent polyester / ammonia blended fabric, and heating the fabric at 80° C. for 4 min to obtain a fabric modified by a charge effect modifier;

[0095] (3) coating the rice microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0096] (4) The fabric containing the nano-microspheres is placed in an oven at 120° C. and heated for 20 min to obtain a textile with an irregular photonic crystal texture pattern.

[0097] Example 8

[0098] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0099] (1) Preparation of nano-microsphere printing paste: a PS@P (MMA-BA) nano-microsphere dispersion having a particle size of 310 nm and a mass fraction of 45% is mixed with 2% propylene glycol, 0.16% nano carbon black, and 5% fatty alcohol polyoxyethylene ether, based on the weight of the nano-microsphere dispersion being 100%, and the mixture is set aside;

[0100] (2) coating a 6% sodium dodecyl sulfate aqueous solution on the surface of a white water-repellent finished polyester fabric, and then heating it at 80° C. for 4 minutes to obtain a fabric modified by a charge effect modifier;

[0101] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0102] (4) The fabric containing the nano-microspheres was placed in an oven at 120° C. and heated for 15 min to obtain a textile with an irregular photonic crystal texture pattern.

[0103] Example 9

[0104] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0105] (1) preparing nano-microsphere printing paste: uniformly mixing SiO2 nano-microsphere dispersion liquid with a particle size of 260 nm and a mass fraction of 25%, 1% glycerol, 0.20% nano carbon black, and 3% polyoxyethylene sorbitan fatty acid ester based on 100% of the weight of the nano-microsphere dispersion liquid, and setting aside;

[0106] (2) coating a 6% sodium dodecyl sulfate aqueous solution on the surface of a white polyester fabric with a special polymer film, and then heating it at 80° C. for 4 minutes to obtain a fabric modified by a charge effect modifier;

[0107] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0108] (4) The fabric containing the nano-microspheres was placed in an oven at 60° C. and heated for 50 min to obtain a textile with an irregular photonic crystal texture pattern.

[0109] Example 10

[0110] A method for preparing a textile with an irregular photonic crystal texture pattern, the specific steps are as follows:

[0111] (1) Preparation of nano-microsphere printing paste: a PS nano-microsphere dispersion having a particle size of 245 nm and a mass fraction of 30% is mixed with 3% propylene glycol, 0.3% nano carbon black, and 5% fatty alcohol polyoxyethylene ether, based on 100% by weight of the nano-microsphere dispersion, and the mixture is set aside;

[0112] (2) coating a 0.3% carboxymethyl cellulose aqueous solution on the surface of a white polyester fabric with a special polymer film to obtain a fabric modified by a charge effect modifier;

[0113] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the modified fabric;

[0114] (4) The fabric containing the nano-microspheres was placed in an oven at 50° C. and heated for 60 min to obtain a textile with an irregular photonic crystal texture pattern.

[0115] Figure 1 , 3The digital photos of textiles with irregular photonic crystal texture patterns prepared in Examples 1 and 3 respectively, are shown. The fabrics are modified by charge effect using anionic surfactants. Due to the principle that like charges repel each other, charged colloidal nanospheres are locally enriched and supersaturated and crystallized on the textile substrate modified by the charge effect modifier, forming irregular photonic crystal texture patterns, proving that anionic surfactants can be used as fabric charge effect modifiers.

[0116] Figure 2 This is a digital photo of the textile with irregular photonic crystal texture pattern prepared in Example 2 and its reflectivity curve. As shown in the reflectivity curve, the reflection peak in the texture pattern area is high and narrow, proving that its structural color brightness and saturation are high.

[0117] Figure 4 This is a digital photograph of a textile with an irregular photonic crystal texture pattern prepared in Example 4. The fabric is modified by charge effect using a cationic surfactant. Due to the principle of attraction between opposite charges, charged colloidal nanospheres are locally enriched and supersaturated and crystallized on the textile substrate modified by the charge effect modifier, forming an irregular photonic crystal texture pattern, proving that cationic surfactants can be used as fabric charge effect modifiers.

[0118] Figure 5 , 6 10 are digital photographs of textiles with irregular photonic crystal texture patterns prepared in Examples 5, 6, and 10, respectively. The fabrics are modified by using charged natural or synthetic polymers. Due to the principle of like charges repelling each other and the "fencing" effect of polymers, even if extremely low concentrations (less than 0.8%) of polymer charge effect modifiers are used, the charged colloidal nanospheres are significantly enriched and supersaturated and crystallized on the textile substrate modified by the polymer charge effect modifier to form irregular photonic crystal texture patterns, proving that charged natural or synthetic polymers can be used as efficient fabric charge effect modifiers.

[0119] Figure 7 , 8 , 9 are digital photos of textiles with irregular photonic crystal texture patterns prepared in Examples 7, 8, and 9, respectively. It can be seen from the figures that the textiles with irregular photonic crystal texture patterns prepared have obvious iridescent effects.

[0120] Comparative Example 1

[0121] (1) Preparation of nano-microsphere printing paste: a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 310 nm and a mass fraction of 45% is mixed with 2% propylene glycol, 0.16% nano carbon black, and 7% fatty alcohol polyoxyethylene ether, based on the weight of the nano-microsphere dispersion being 100%, and the mixture is set aside;

[0122] (2) coating the nano-microsphere printing paste prepared in step (1) on the surface of a white polyester fabric that has been treated with water repellent finishing;

[0123] (3) The fabric containing the nano-microspheres was placed in an oven at 120° C. and heated for 15 min to obtain a textile with an irregular photonic crystal texture pattern.

[0124] Comparative Example 2

[0125] (1) Preparation of nano-microsphere printing paste: a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 255 nm and a mass fraction of 35% is mixed with 1% propylene glycol, 0.20% nano carbon black, and 4% fatty alcohol polyoxyethylene ether, based on the weight of the nano-microsphere dispersion being 100%, and the mixture is set aside;

[0126] (2) coating a 6% aqueous solution of fatty alcohol polyoxyethylene ether on the surface of a white water-repellent finished polyester fabric, and then heating it at 80° C. for 4 minutes;

[0127] (3) coating the nano-microsphere printing paste prepared in step (1) on the surface of the fabric treated in step (2);

[0128] (4) The fabric containing the nanospheres was placed in an oven at 120°C and heated for 20 min to obtain a textile without a texture pattern.

[0129] Comparative Example 3

[0130] (1) preparing nano-microsphere printing paste: a PS@P(MMA-EA) nano-microsphere dispersion having a particle size of 256 nm and a mass fraction of 45% is mixed with 5% propylene glycol, 0.22% water-soluble black pigment, and 6% fatty acid polyoxyethylene ester, based on 100% of the weight of the nano-microsphere dispersion, and the mixture is set aside;

[0131] (2) coating a 0.4% sodium polyacrylate aqueous solution on the surface of a white hydrophilic cotton fabric that has not been water-repellent finished;

[0132] (3) applying the nano-microsphere printing paste prepared in step (1) on the surface of the fabric treated in step (2);

[0133] (4) The fabric containing the nanospheres was placed in an oven at 90°C and heated for 30 min to obtain a textile without a texture pattern.

[0134] Comparative Example 4

[0135] (1) Preparation of nano-microsphere printing paste: a PS@P(MMA-BA) nano-microsphere dispersion having a particle size of 188 nm and a mass fraction of 46% is mixed with 6% propylene glycol and 7% fatty alcohol polyoxyethylene ether based on 100% of the weight of the nano-microsphere dispersion, and the mixture is set aside;

[0136] (2) coating a 0.2% sodium alginate aqueous solution on the surface of a black hydrophilic cotton fabric that has not been water-repellent finished, and heating it at 80° C. for 4 min;

[0137] (3) applying the nano-microsphere printing paste prepared in step (1) on the surface of the fabric treated in step (2);

[0138] (4) The fabric containing the nanospheres was placed in an oven at 110°C and heated for 25 min to obtain a textile without a texture pattern.

[0139] Comparative Example 5

[0140] (1) Preparation of nano-microsphere printing paste: a PS nano-microsphere dispersion having a particle size of 245 nm and a mass fraction of 30% is mixed with 3% propylene glycol, 0.3% nano carbon black, and 5% fatty alcohol polyoxyethylene ether, based on 100% by weight of the nano-microsphere dispersion, and the mixture is set aside;

[0141] (2) coating a 5% carboxymethyl cellulose aqueous solution on the surface of a white polyester fabric with a special polymer film to obtain a fabric modified by a charge effect modifier;

[0142] (3) applying the nano-microsphere printing paste prepared in step (1) on the surface of the fabric treated in step (2);

[0143] (4) The fabric containing the nanospheres was placed in an oven at 50°C and heated for 60 minutes to obtain a textile without a texture pattern.

[0144] Fig.11 This is a digital photograph of a textile without a texture pattern prepared in Comparative Example 1 (compared with Example 8). When the fabric is not modified by a charge effect modifier, there is no significant electrostatic interaction between the fabric and the nano-microspheres, and an irregular photonic crystal pattern cannot be generated.

[0145] Fig.12 This is a digital photograph of a textile without a texture pattern prepared in Comparative Example 2 (compared with Example 7). When a non-ionic surfactant is used as a charge effect modifier to modify the fabric, there is no charge effect between it and the nano-microspheres, and an irregular photonic crystal pattern cannot be generated.

[0146] Fig.13This is a digital photo of a textile without a texture pattern prepared in Comparative Example 3 (compared with Example 6). When the hydrophilic cotton fabric is not subjected to water-repellent finishing, the charge effect modifier and the nano-microsphere printing paste will penetrate into the back of the fabric, the brightness and saturation of the fabric are low, and no obvious irregular photonic crystal texture pattern can be produced.

[0147] Fig.14 This is a digital photo of a textile without a texture pattern prepared in Comparative Example 4 (compared with Example 5). After the surface of the fabric is coated with an aqueous sodium alginate solution and then heated, since there is less water in the nano-microsphere printing slurry, it is difficult for the sodium alginate to completely swell and ionize, and it is difficult to produce a strong charge effect with the nano-microspheres, so an irregular photonic crystal pattern cannot be produced.

[0148] Fig.15 This is a digital photo of a textile without a texture pattern prepared in Comparative Example 5 (compared with Example 10). When the concentration of the carboxymethyl cellulose aqueous solution is too high, since carboxymethyl cellulose is a polymer, its excessive amount will hinder the orderly assembly of the photonic crystals, and the brightness and saturation of the prepared fabric are low, and no obvious irregular photonic crystal texture pattern can be produced.

[0149] In summary, the present invention utilizes the basic physical principle that like charges repel each other and opposite charges attract each other, promoting the local enrichment and supersaturated crystallization of charged colloidal nanospheres on a textile substrate modified by a charge effect modifier, forming an irregular photonic crystal texture pattern, and obtaining a textile having both a unique texture pattern and an iridescent effect structural color, so that the pattern of each textile product is unique.

[0150] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0151] The above is a detailed introduction to a textile with an irregular photonic crystal texture pattern and a preparation method thereof provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a textile having an irregular photonic crystal texture pattern, Features The method comprises the following steps: S1. Preparation of nano-microsphere printing paste The nanosphere dispersion, the high boiling point additive, the stray light absorber and the surfactant are uniformly mixed to obtain the nanosphere printing paste; wherein the solid content of the nanosphere dispersion is 25% to 55%; based on the weight of the nanosphere dispersion as 100%, the amount of the high boiling point additive is 0.5 to 6% of the weight of the nanosphere dispersion, the amount of the stray light absorber is 0 to 0.3% of the weight of the nanosphere dispersion, and the amount of the surfactant is 2 to 8% of the weight of the nanosphere dispersion; The high boiling point additive is selected from one or a mixture of glycerol, propylene glycol, formamide, and ethylene glycol; The surfactant is selected from one or a mixture of fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene sorbitan fatty acid ester, fatty acid methyl ester ethoxylate or ethylene oxide adduct of polypropylene glycol; The stray light absorber is selected from one or a mixture of black dye, nano carbon black or water-soluble black pigment; S2, applying an aqueous solution of a charge effect modifier on the surface of a hydrophobic fabric, and performing subsequent heating and drying / non-heating and drying treatment according to the performance and application method of the charge effect modifier to obtain a modified fabric; The charge effect modifier is an ionic surfactant or a charged polymer. When the charge effect modifier is an ionic surfactant, the concentration is 0.1-30 wt %; when the charge effect modifier is a charged polymer, the concentration is 0.01-0.8 wt %; S3, applying nano-microsphere printing paste on the surface of the modified fabric obtained in S2; S4. The modified fabric containing the nano-microsphere coating obtained in S3 is heated and assembled to obtain a textile having an irregular photonic crystal texture pattern.

2. The preparation method according to claim 1, Features: The nanoparticles described in S1 are colloidal nanoparticles with ionic groups or negatively or positively charged surfaces, including Organic polymer colloidal nanospheres: polystyrene (PS), polymethyl methacrylate (PMMA), polystyrene@polyacrylic acid (PS@PAA), polystyrene@polydopamine (PS@PDA), poly(styrene-hydroxyethyl acrylate) (P(St-HEA)), poly(styrene-methyl methacrylate) (P(St-MMA)), poly(styrene-methacrylic acid) (P(St-MAA)), polystyrene@poly(methyl methacrylate-butyl acrylate) (PS@P(MMA-BA)), polymethyl methacrylate@poly(hydroxyethyl acrylate-hydroxyethyl methacrylate) (PMAA@P(HEA-HEMA)), poly(styrene-methacrylic acid)@poly(ethyl acrylate-methacrylic acid) (P(St-MAA)@P(EA-MAA)) nanospheres, Inorganic colloidal nano-microspheres of silica (SiO 2 ), titanium dioxide (TiO 2 ), zirconium oxide (ZrO) nanospheres, or Organic@inorganic and inorganic@organic colloidal nanoparticles of polystyrene@silica (PS@SiO 2 ), silicon dioxide@polystyrene (SiO 2 @PS) Any one of the nanoparticles.

3. The preparation method according to claim 1, Features: The ionic surfactants in S2 include anionic surfactants and cationic surfactants, the anionic surfactants include sodium stearate, sodium palmitate, sodium dodecyl sulfate or sodium dodecylbenzene sulfonate; the cationic surfactants include hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide or hexadecylpyridinium chloride; the charged natural or synthetic polymers include sodium alginate, carboxymethyl cellulose, sodium polyacrylate and their derivatives.

4. The preparation method according to claim 1, Features: The charge effect modifier in S2 is applied by dipping, padding or coating.

5. The preparation method according to claim 1, Features: The subsequent heating and drying / non-heating drying treatment described in S2 is carried out according to the performance and application method of the charge effect modifier. Specifically, when an ionic surfactant is used, the modified fabric needs to be heated and dried at a temperature of 60~90°C and a drying time of 2~5min. When a charged polymer is used, the liquid carrying rate of the modified fabric is controlled to be 5~80% without heating and drying treatment, and the next step of processing is directly carried out.

6. The preparation method according to claim 1, Features: The hydrophobic fabric described in S2 has a water contact angle of 110° to 180°.

7. The preparation method according to claim 1, Features: The nano-microsphere printing paste described in S3 is applied by blade coating or spraying.

8. The preparation method according to claim 1, Features: The heating assembly described in S4 has an assembly temperature of 40 to 130° C. and an assembly time of 3 to 60 minutes.

9. The preparation method according to claim 1, Features: The fabric is selected from polyester fabric, nylon fabric, cotton fabric, silk fabric, polyester-cotton blended fabric or polyester-spandex blended fabric.

10. A textile having an irregular photonic crystal texture pattern obtained according to the preparation method of claim 1.

Citation Information

Patent Citations

  • Preparation method of surface adsorption dye type nano microsphere structure chromogenic ink for textile digital jet printing self-assembly

    CN108442138A

  • Large-area preparation method of high-stability high-saturation photonic crystal structure yarn-producing fabric

    CN114164661A

  • Rapid large-area preparation method of bionic photonic crystal structure yarn-producing fabric

    CN115094645A

  • Photonic crystal structural color material based on natural polymer material and preparation method thereof

    CN118444413A

  • Method of fabricating photonic crystal

    KR1020140059579A