Method for detecting single-stage aging precipitated phase and fatigue performance of aluminum alloy

Through jet deposition technology and single-stage aging treatment, combined with fatigue test and transmission electron microscopy, the problems of single-stage aging phase and fatigue performance detection in aluminum alloy materials are solved, and the crack resistance and fatigue strength of aluminum alloys are improved.

CN119086318APending Publication Date: 2024-12-06INNER MONGOLIA UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222588.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively detect the single-stage aging phase and fatigue properties of aluminum alloys, resulting in the accumulation damage and fatigue strength of the material under long-term strain and alternating loads, affecting the material's crack propagation ability.

Method used

The aluminum alloy material is completely melted and heat treated in a vacuum furnace by spray deposition technology, followed by a single-stage aging treatment, and the fatigue performance and precipitation phases of multiple aging times are detected by equipment such as fatigue testing machines and transmission electron microscopes.

Benefits of technology

By analyzing the fatigue properties and precipitation phases of the aluminum alloy, combined with data under different temporal efficiency states, the fatigue properties of the aluminum alloy are improved, the crack resistance is improved, and the long-term service performance of the material is optimized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119086318A_ABST
    Figure CN119086318A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum alloy single-stage aging precipitated phase and fatigue performance detection method which comprises the following steps: putting an aluminum alloy material into a vacuum melting furnace, completely melting the aluminum alloy material, preserving the heat to obtain liquid metal, preparing the liquid metal into a deposited alloy by using a spraying immediate machine device, and carrying out heat treatment; performing single-stage aging treatment on the aluminum alloy subjected to heat treatment; detecting the fatigue performance of the aluminum alloy in a plurality of aging times; and detecting the precipitated phases of the aluminum alloy in multiple aging times. According to the method, the single-stage aging fatigue performance and the precipitated phase of the aluminum alloy are detected, the fatigue performance and the precipitated phase of the aluminum alloy are analyzed respectively, and different single-stage aging fatigue performance and precipitated phase data are analyzed and combined, so that the fatigue performance of the aluminum alloy is improved, and the crack propagation resistance of the aluminum alloy is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy material detection technology, in particular to a method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy. Background Art

[0002] As a high-strength, precipitation-hardened, heat-treatable aluminum alloy, spray-deposited 7055 aluminum alloy has been widely used in the aviation and military industries due to its ultra-high strength-to-weight ratio, fracture toughness, and resistance to stress corrosion cracking. After artificial heat treatment, the fatigue properties of the alloy change significantly. Different microstructures: grain size, second phase, grain boundary, etc. will lead to different fatigue crack growth behaviors. With the development of science and technology, the requirements for the comprehensive properties of aluminum alloys, especially fatigue properties, are becoming higher and higher. Under the action of long-term strain and alternating loads, the long-term accumulated damage will eventually lead to material fracture, and as the crack growth rate increases, the fatigue strength will also increase.

[0003] For aluminum alloys, most alloys used in engineering are aged alloys. Therefore, after the alloy is aged, the precipitation phase becomes an important factor affecting the alloy performance. At the same time, the fatigue performance of aluminum alloys is the ability of aluminum alloys to resist crack growth. The fatigue life of aluminum alloys under different aging conditions is significantly different. Therefore, it is necessary to test the single-stage aging precipitation phase and fatigue performance of aluminum alloys. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy to solve the problems raised by the above-mentioned background technology.

[0005] The technical solution adopted by the present invention to solve the technical problem is: a method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy, comprising the following steps:

[0006] The aluminum alloy material is placed in a vacuum furnace to completely melt the aluminum alloy material and then kept warm to obtain liquid metal, and the liquid metal is sprayed with a spraying device to obtain a deposited alloy, and then heat-treated;

[0007] Single-stage aging treatment of heat-treated aluminum alloys;

[0008] Test the fatigue properties of aluminum alloys at multiple aging times;

[0009] The precipitation phase of aluminum alloy with multiple aging times was detected.

[0010] As a further improvement of the present invention: placing the alloy material into a vacuum melting furnace to completely melt the alloy material and then keeping the temperature includes: the alloy material is completely melted in a vacuum furnace at 820° C. to 880° C. and then keeping the temperature for 10 minutes.

[0011] As a further improvement of the present invention: the method of preparing a deposited alloy from liquid metal using a jet deposition device comprises: preparing a columnar deposited alloy with a diameter of 180 mm and a height of 400 mm using a jet deposition device, selecting a columnar deposited alloy with a central portion having a diameter of 100 mm and a height of 200 mm for hot extrusion, and obtaining a rod alloy with a diameter of 40 mm.

[0012] As a further improvement of the present invention: the single-stage aging treatment of the heat-treated aluminum alloy includes a single-stage aging treatment of the rod alloy at 120°C.

[0013] As a further improvement of the present invention: the multiple aging times include an under-aging UA state, a peak-aging PA state and an over-aging OA state, the holding time of the under-aging UA state is 2 hours, the holding time of the peak-aging PA state is 10 hours, and the holding time of the over-aging OA state is 40 hours.

[0014] As a further improvement of the present invention: the fatigue performance of the aluminum alloy is tested, including: using a fatigue testing machine to perform a tension-compression fatigue test, the stress level is 300MPa, the frequency is 10HZ, the stress ratio R=01, the load type is a sine wave, and the fatigue test is performed in an atmospheric environment at room temperature.

[0015] As a further improvement of the present invention: the fatigue performance testing of the aluminum alloy also includes: sampling the fatigue specimens for the fatigue performance testing of the aluminum alloy along the extrusion direction of the extruded rod, grinding and polishing the cross-section of the specimen of the extruded rod alloy with sandpaper, observing the specimen with a field emission scanning electron microscope at 20 kV, and performing microstructural analysis and characterization on the extruded alloy.

[0016] As a further improvement of the present invention: the fatigue performance testing of the aluminum alloy also includes: placing multiple aged aluminum alloy sample discs into an MT-PI type ion double-jet electrolytic thinning instrument to thin the samples, the electrolyte is 30% HNO3+70% CH3OH, the temperature of the thinning liquid is monitored and controlled at -30°C to -20°C using a thermometer, the current is controlled at 100-120mA, the voltage is 15-20V, and the microstructures of the multiple aged aluminum alloys are observed by transmission electron microscopy at 200kV.

[0017] As a further improvement of the present invention: the detection of the precipitation phase of the aluminum alloy at multiple aging times includes: using a transmission electron microscope to observe the TEM bright field image of the aluminum alloy at different aging times at 120°C.

[0018] As a further improvement of the present invention: the detection of the precipitation phase of the aluminum alloy at multiple aging times also includes: observing the SAED pattern of the crystal band axis of the aluminum alloy at different aging times at 120°C using a transmission electron microscope.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention utilizes the detection of fatigue performance and precipitation phase of aluminum alloy in single-stage aging, analyzes the fatigue performance and precipitation phase of aluminum alloy respectively, and combines the phase analysis of different single-stage aging fatigue performance and precipitation phase data, which helps to improve the fatigue performance of aluminum alloy and enhance the crack growth resistance of aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the process of the present invention.

[0022] Figure 2 Hardening curve of spray-formed 7055 extruded aluminum alloy during aging treatment at 120°C.

[0023] Figure 3 This is a diagram of the mechanical properties of spray-formed 7055 extruded aluminum alloy under different aging conditions.

[0024] Figure 4 The macroscopic morphology of fatigue fracture of spray-formed 7055 aluminum alloy after aging treatment with different aging times.

[0025] Figure 5 The morphology of fatigue crack initiation position of spray-formed 7055 aluminum alloy after aging treatment with different aging times.

[0026] Figure 6 The morphology of the first stage of fatigue crack growth in spray-formed 7055 aluminum alloy after aging treatment with different aging times.

[0027] Figure 7 The second stage morphology of fatigue crack growth in spray-formed 7055 aluminum alloy after aging treatment with different aging times.

[0028] Figure 8 These are the morphologies of the fatigue instantaneous fracture zone of spray-formed 7055 aluminum alloy after aging treatment for different aging times.

[0029] Fig. 9 TEM bright field images of 7055 aluminum alloy at different aging times.

[0030] Fig.10 SAED patterns of

[011] Al and

[112] Al crystal axis of 7055 aluminum alloy after aging at 120℃ for different times. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0032] Since the fatigue properties of alloys change significantly after artificial heat treatment, different microstructures: grain size, second phase, grain boundary, etc. will lead to different fatigue crack growth behaviors. For aluminum alloys, most alloys used in engineering are aged alloys. Therefore, after the alloy is aged, the precipitation phase becomes an important factor affecting the performance of the alloy. Reasonable regulation of the type, quantity, size, and distribution of the precipitation phase becomes a key means to ensure that components can serve long-term and safely.

[0033] The present invention is further described in conjunction with the accompanying drawings and embodiments: A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy comprises the following steps:

[0034] The aluminum alloy material is placed in a vacuum furnace to completely melt the aluminum alloy material and then kept warm to obtain liquid metal, and the liquid metal is sprayed with a spraying device to obtain a deposited alloy, and then heat-treated;

[0035] Single-stage aging treatment of heat-treated aluminum alloys;

[0036] Test the fatigue properties of aluminum alloys at multiple aging times;

[0037] The precipitation phase of aluminum alloy with multiple aging times was detected.

[0038] In one embodiment of the present application, placing the alloy material into a vacuum furnace to completely melt the alloy material and then keeping it warm includes: completely melting the alloy material in a vacuum furnace at 820° C. to 880° C. and then keeping it warm for 10 minutes.

[0039] In one embodiment of the present application, the method of preparing a deposited alloy from liquid metal using a jet deposition device comprises: preparing a columnar deposited alloy with a diameter of 180 mm and a height of 400 mm using a jet deposition device, selecting a columnar deposited alloy with a center diameter of 100 mm and a height of 200 mm for hot extrusion, and obtaining a rod alloy with a diameter of 40 mm.

[0040] The experimental alloy used was a spray-deposited high-zinc Al-Zn-Mg-Cu alloy, the chemical composition of which is shown in Table 1. The preparation steps of the alloy were as follows: the alloy was completely melted in a vacuum furnace at 820°C to 880°C and then kept warm for 10 minutes, a columnar deposited alloy with a diameter of 180 mm and a height of 400 mm was prepared using a spray deposition device, and a columnar deposited alloy with a center diameter of 100 mm and a height of 200 mm was selected for hot extrusion to obtain a rod with a diameter of 40 mm.

[0041] In a comparative example, the extruded bar was subjected to a two-stage solution treatment at 440°C / 4h+490°C / 30min, and water quenched at room temperature, with a transfer time of less than 15s. After being stored at room temperature for 48h, the solution treated alloy was kept at 120°C.

[0042] Table 1 Chemical composition of the test alloys (wt.%)

[0043] Tablel The chemical composition of experimental alloy(wt.%)

[0044]

[0045] In one embodiment of the present application, the single-stage aging treatment of the heat-treated aluminum alloy includes subjecting the rod alloy to a single-stage aging treatment at 120°C.

[0046] The evolution of the precipitate phase of the spray-deposited A112Zn2.4Mg1.1Cu alloy was studied. After the experimental alloys were aged at 120, 140 and 160℃, their hardness curves were analyzed and it was found that the hardness showed an obvious "double peak" when aged at 120℃, and the hardness after aging at 140 and 160℃ was relatively low, so the aging temperature was selected as 120℃.

[0047] In one embodiment of the present application, the multiple aging states include an under-aging UA state, a peak-aging PA state, and an over-aging OA state. The holding time of the under-aging UA state is 2 hours, the holding time of the peak-aging PA state is 10 hours, and the holding time of the over-aging OA state is 40 hours.

[0048] like Figure 2 The figure below shows the relationship between hardness and aging time after the alloy has been treated with a single-stage aging treatment at 120°C. Figure 2 Select appropriate holding time for under-aging, peak aging and over-aging, by Figure 2It can be seen that after aging for 2 hours, the hardness of the test alloy has reached 220.1HV. In the first two hours of aging, the hardness increases fastest with the increase of aging time, and the slope is the largest. After aging for 4 hours, the hardness value of the alloy is 238.5HV, and the hardness continues to increase, indicating that the test alloy has a very fast aging response characteristic. Figure 2 It can be clearly seen that the hardness value of the alloy presents a "double peak" phenomenon. When the aging time reaches 10h, the hardness of the alloy is 254.6HV, and the hardness reaches the peak value. With the increase of aging time, the hardness of the alloy does not continue to rise. As the aging time continues, the hardness value shows a downward trend. When the aging time is 32h, the hardness of the alloy drops to 235.1HV. Therefore, as the aging time increases, the hardness of the test alloy treated with single-stage aging at 120℃ first increases rapidly, and then rises to the maximum value relatively slowly. When the test alloy reaches the peak hardness, it drops rapidly to a certain extent. Subsequently, as the aging time increases, the hardness of the test alloy fluctuates within a range. Since the hardness and strength of the alloy are linearly related, the change in strength can be selected with reference to the change in hardness. Therefore, aging times of 2h, 10h, and 40h are selected as the under-aging (UA state), peak aging (PA state), and over-aging (OA state) of the spray-formed 7055 aluminum alloy extruded bar, respectively.

[0049] In one embodiment of the present application, the fatigue performance testing of the aluminum alloy includes: using a fatigue testing machine to perform a tension-compression fatigue test, the stress level is 300MPa, the frequency is 10HZ, the stress ratio R=01, the load type is a sine wave, and the fatigue test is performed in an atmospheric environment at room temperature.

[0050] In one embodiment of the present application, the fatigue performance testing of the aluminum alloy also includes: sampling fatigue specimens for fatigue performance testing of the aluminum alloy along the extrusion direction of the extruded rod, grinding and polishing the cross-section of the specimen of the extruded rod alloy with sandpaper, observing the specimen with a field emission scanning electron microscope at 20 kV, and performing microstructural analysis and characterization on the extruded alloy.

[0051] Furthermore, the fatigue performance testing of the aluminum alloy also includes: placing multiple aged aluminum alloy sample discs into an MT-PI type ion double-jet electrolytic thinning instrument to thin the samples, the electrolyte is 30% HNO3+70% CH3OH, the temperature of the thinning liquid is monitored and controlled at -30°C to -20°C using a thermometer, the current is controlled at 100-120mA, the voltage is 15-20V, and the microstructures of the multiple aged aluminum alloys are observed by transmission electron microscopy at 200kV.

[0052] The cross-sections of the extruded and solid solution alloy samples were polished with 80# to 2500# sandpaper, and the polished specimens were placed in the p-3 type polishing process until there were no scratches on the mirror surface. Then, the samples were observed under a field emission scanning electron microscope at 20kV, and the microstructures of the extruded alloys and the aged alloys were analyzed and characterized. The microstructures of the three aged aluminum alloys were observed under TEM at 200kV using a transmission electron microscope (resolution of 0.2nm). The prepared thin sheets were punched into discs with a diameter of 3mm. In the process of punching the discs, it is necessary to avoid improper operation of the thin sheets to produce bulges or bends, which will cause stress concentration and affect the later use. The punched 3mm discs were placed in the MT-PI ion double-jet electrolytic thinning instrument to thin the samples. The electrolyte is 30% HNO3 + 70% CH3OH. The temperature of the thinning liquid is monitored by a thermometer at -30 to -20°C. The current should be controlled at 100-120mA and the voltage at 15-20V.

[0053] according to Figure 3 The mechanical properties diagram of the spray-formed 7055 aluminum alloy extruded bar in three aging states: under-aging UA state, peak aging PA state, and over-aging OA state.

[0054] from Figure 3 It can be clearly seen that after aging treatment, the tensile strength and yield strength of the three aged alloys are significantly improved compared with the alloys after 440℃ / 4h+490℃ / 30min double-stage solid solution treatment. The tensile strength and yield strength of the alloy after 440℃ / 4h+490℃ / 30min double-stage solid solution treatment are 559MPa and 517MPa respectively. Figure 3 It can be obtained that the hardness increases fastest when the aging time is 2h, and the tensile strength and yield strength are 679MPa and 620MPa respectively. In the early stage of aging, the hardness and strength increase very quickly. This is because the alloy has significant aging response characteristics. At the initial aging time of 2h, a large amount of strengthening phases will precipitate in the 7055 aluminum alloy, which can significantly improve the mechanical properties of the alloy. When the aging time is 10h, the hardness and strength of the alloy both reach the peak value. At this time, the tensile strength and yield strength of the alloy are 729MPa and 688MPa respectively. The types of second phases precipitated in the alloy are increasing, and the strengthening effect on the alloy is becoming more and more significant. When the aging time is 40h, the yield strength and tensile strength both show a downward trend. At this time, the tensile strength and yield strength of the alloy are 690MPa and 632MPa respectively. This is mainly because with the extension of the aging time, some second phases appear coarsening, and the number of fine second phases decreases, resulting in a decrease in the hardness and strength of the alloy, but its elongation is higher than that of the PA state alloy, about 12.5%.

[0055] Table 2 shows the fatigue life values ​​of the spray-formed 7055 aluminum alloy in UA, PA, and OA states. The dimensional error of each group of three fatigue specimens does not exceed 0.1 mm. Under the maximum stress of 300 MPa and the stress ratio R = 0.1, a tension-compression fatigue test is carried out, and the average value of the fatigue life of the three parallel specimens is taken to represent the fatigue life (times) of the alloy in this state. As can be seen from Table 2, the average fatigue life of the OA alloy is significantly higher than that of the UA and PA alloys, which is 222,000 times, indicating that the fatigue performance of the OA alloy is better than that of the PA alloy, followed by the UA alloy, and the fatigue life under different aging conditions is significantly different.

[0056] Table 2 Fatigue life of spray-formed 7055 aluminum alloy at different aging states at 300 MPa

[0057] Table2 Fatigue life of spray formed 7055aluminum alloy under different aging conditions at 300MPa

[0058]

[0059] Figure 4 In the figure, (a), (b), and (c) are the fatigue fracture macroscopic morphologies of UA, PA, and OA spray-formed 7055 aluminum alloy. Figure 4It can be seen that the morphology of the fracture can be divided into three main areas: fatigue crack source area, fatigue crack extension area, and fatigue instantaneous fracture area. The fatigue crack initiation area is usually located on the surface of the material or near the surface, and is connected with the crack extension area to form a radial pattern. Among the three areas, the fatigue crack extension area usually shows a relatively flat surface. This flatness is mainly due to the fact that the formation process of this area takes a long time and is gradually formed under the action of multiple cycles of stress. In contrast, the formation process of the fatigue instantaneous fracture area is relatively rapid, and usually the material suddenly breaks after it is subjected to the ultimate stress. The flatness of the fatigue crack extension area is also related to the low expansion rate during its formation process. Since the crack expands slowly in this area, there is enough time to form a relatively smooth crack path on the surface of the material. This slow expansion process allows the material to gradually undergo plastic deformation under stress, thereby forming a relatively flat feature on the fracture surface. However, due to its rapid fracture characteristics, the fatigue instantaneous fracture area is usually accompanied by a relatively rough and irregular fracture surface. When the crack expands to a certain extent, the remaining strength of the material is not enough to support the material to continue fatigue, and the material will break instantly. By observing the instantaneous fracture zone, it can be found that the fracture surface of the instantaneous fracture zone is rougher than that of the crack extension zone and the fatigue source zone. In the entire fatigue process, the fatigue instantaneous fracture zone occupies the largest area. The tearing edge can be clearly seen in the alloys of the three states, and the tearing edge of the UA state alloy is the most obvious.

[0060] Figure 5 In the figure, (a), (b), and (c) are the morphological images of the fatigue crack initiation positions of UA, PA, and OA spray-formed 7055 aluminum alloys. It can be clearly seen from the figure that the crack propagation process usually takes the crack source as the center point and then spreads to the surrounding areas to form a radial pattern. This crack source area mainly appears on the surface of the material or close to the surface. When the material undergoes a fatigue process, it will be subjected to periodic loads. During this process, some larger second-phase particles may hinder the movement of dislocations, causing dislocations to accumulate around the particles and form stress concentration points. This stress concentration may eventually cause the interface between the second phase and the matrix material to separate, thereby forming tiny holes at the interface. As the fatigue process continues, these holes gradually develop into the starting points of cracks. Under long-term cyclic loads, these initial hole positions will gradually expand to form cracks. These cracks will expand along a specific path inside the material over time and with the accumulation of stress, eventually leading to the fracture of the material. The stress concentration and hole formation caused by the second phase particles are one of the key factors in the formation and development of fatigue cracks. These second phase particles are mostly metal oxides or Fe-rich phases.

[0061] Figure 6In the figure, (a), (b), and (c) are the first stage morphologies of fatigue crack growth of 7055 aluminum alloy spray-formed in UA, PA, and OA states. Figure 6 It can be found that there are many tiny protrusions and cliffs on the fatigue fracture surface. These characteristic structures are neatly arranged along the direction of crack propagation, forming an orderly distribution pattern. The formation of this feature is closely related to the mechanism of crack propagation inside the material. When a crack propagates from one grain to another, if the slip system directions of the two grains are consistent, the crack can smoothly pass through the grain boundary and enter the interior of the adjacent grain. However, if the slip system directions of the two grains are inconsistent and there is a certain angle difference, the crack propagation path may be affected. In this case, the crack may turn to other adjacent grains that are conducive to its propagation, or stop propagating when encountering obstacles. Figure 6 It can be seen that the UA alloy has many large and deep holes. These holes gradually expand and increase with the continuation of fatigue cycles, forming Figure 6 The holes seen in the OA alloy. The formed holes not only weaken the bearing capacity of the material, but also provide a starting point for the initiation and propagation of cracks. During the fatigue process, these holes may develop into crack sources, further aggravating the damage of the material. The holes in the OA alloy are less than those in the UA alloy because the strengthening phase precipitated in the OA alloy enhances the crack resistance and ductility of the alloy.

[0062] The first stage of fatigue crack growth is the transition period from fatigue source area to crack growth. Then the crack growth will enter the second stage, which is the stable period of crack growth. Figure 7 In the figure, (a), (b), and (c) show the second stage morphology of fatigue crack growth of 7055 aluminum alloy spray-formed in UA, PA, and OA states. Figure 7 In the figure, (d), (e), and (f) are partial enlarged images of (a), (b), and (c). The fatigue striations unique to fatigue can be clearly seen in the figure. These striations are a significant feature of the crack propagation process when the material undergoes cyclic loading stress. Every time the specimen is subjected to a cyclic loading, the front of the crack will experience a sharpening, leaving a clear striation on the fracture surface. The formation of these striations is direct evidence of the crack propagation in each stress cycle, and each fatigue striation corresponds to a complete stress cycle. Figure 7 In (f), it can be observed that many secondary cracks are generated in the fatigue stripes of the OA state alloy. These tiny cracks are parallel to the original fatigue cracks. The depth of the secondary cracks is significantly greater than the traces formed by the fatigue stripes. The generation of secondary cracks will reduce the crack propagation rate. Figure 7It can also be seen that during the fatigue crack propagation process, part of the second phase falls off from the matrix to form a large number of holes. This is mainly because under the action of cyclic stress loading, due to the obstruction of the second phase, dislocation pile-up will form near the second phase, resulting in stress concentration and part of the second phase falling off from the matrix surface.

[0063] Figure 8 In the figure, (a), (b), and (c) are the morphologies of fatigue instantaneous fracture zones of 7055 aluminum alloys spray-formed in UA, PA, and OA states. The instantaneous fracture modes of the alloys in the three different aging states have common characteristics: they are all mixed fracture modes of dissociation surface and dimple, which are reflected in both brittleness and toughness, and are similar to the morphology of tensile fracture. In the UA and OA alloys, the plastic performance is particularly prominent, which can be seen from Figure 8 It can be clearly seen in (a) and (c). The alloy fractures in these two states are covered with a large number of tiny dimples, and their number exceeds that of the PA alloy. In particular, compared with the PA alloy, the dimples of the OA alloy are not only more numerous, but also larger and deeper. This difference is mainly due to the fact that the plasticity of the alloy has been significantly improved with the deepening of aging treatment.

[0064] In one embodiment of the present application, the detecting of the precipitation phase of the aluminum alloy at multiple aging times includes: using a transmission electron microscope to observe the TEM bright field image of the aluminum alloy at different aging times at 120°C.

[0065] Fig. 9 TEM bright field images of 7055 aluminum alloy at 120℃ for different aging times. Fig. 9 As can be seen from (a), a large number of fine dispersed primary precipitates with a diameter of 2 to 3 nm and a round or oval shape are precipitated in the UA alloy matrix. As the aging time continues to increase, these primary precipitates gradually grow to form larger precipitates with a diameter of about 5 to 7 nm. Fig. 9 (b) is the TEM bright field image of the PA alloy. As the number of precipitated phases increases, the hardness of the alloy gradually increases. After aging at 120℃ / 18h, the alloy reaches a peak hardness of 224.7HV. After aging at 120℃ / 44h, the hardness of the alloy begins to decrease from the peak hardness and eventually stabilizes. Fig. 9 (c) is the TEM bright field image of the OA state alloy. Analysis shows that the precipitate phase has undergone obvious coarsening, the density has decreased, and the diameter of the precipitate phase has coarsened to 9-13nm. The spacing between the precipitates has increased, and the spacing between the precipitates is significantly larger than that of the UA and PA state alloys.

[0066] In one embodiment of the present application, the detection of precipitation phases of aluminum alloys at multiple aging times further includes: observing SAED patterns of the crystal band axis of the aluminum alloy at different aging times at 120° C. using a transmission electron microscope.

[0067] Fig.10 (a), (b), and (c) are 7055 aluminum alloys at 120℃ for different aging times

[011] Al The SAED pattern of the crystal zone axis. <011> Al Diffraction pattern in the direction ( Figure 6 From (a, b, c), it can be seen that the UA alloy has strong continuous bright stripes at {1, (2n + 1) / 4, 0} Al, indicating that the precipitation phase in the crystal is mainly GPⅡ area. At the same time, brighter diffraction spots of L12-Al3Zr phase can also be seen. After single-stage aging treatment at 120℃ / 2h, the formed GPⅡ area is coherent with the aluminum matrix and is cut by dislocations. Fig.10 In (b), the diffraction spots of η′ phase and L12-Al3Zr phase were found. At the same time, the matrix diffraction spots showed bright stripes after aging at 120℃ / 2h, but the brightness was weakened and no longer continuous, indicating that the brightness of the diffraction spots in the GPⅡ zone gradually weakened. Fig. 9 As can be seen from (a) and (b), the growth of the precipitated phase in the PA alloy is not obvious, mainly due to the reduction in the number of small-sized circular or oval GPⅡ zones, and most of the GPⅡ zones in the PA alloy have been transformed into the metastable phase η′. After aging for 40 hours, the precipitated phase in the crystal is mainly η, and some η′ remains. Bright L12-Al3Zr phase diffraction spots are also found, among which the η′ diffraction spots are intermittent, indicating that in the later stage of aging, most of the η′ in the alloy is transformed into a more stable η phase.

[0068] Fig.10 (d), (e), and (f) are samples of 7055 aluminum alloy at 120℃ for different aging times

[112] Al SAED pattern of crystal zone axis. Fig.10 (d) shows that there are faint bright stripes in the diffraction spots of the UA alloy, which are analyzed to be the diffraction spots of the GPⅡ region. At the same time, brighter diffraction spots of the L12-Al3Zr phase are also found. When the PA 7055 alloy is aged for 18 hours, the diffraction spots of the GPⅡ region become discontinuous, and the diffraction spots of the η′ phase become brighter, indicating that part of the GPⅡ region is converted into the η′ phase. Fig.10 (f) is the diffraction spot of OA alloy. It can be seen that the diffraction spot of OA alloy is smaller than that of Fig.10(d) and (e) become more dispersed, indicating that most of the η′ phase in the matrix is ​​transformed into the η phase, and the fixed orientation relationship between the η phase and the matrix disappears. Therefore, the precipitated phase of the OA state alloy is mainly composed of the η phase, and some η′ phase remains.

[0069] Combined with Table 2, it can be seen that the fatigue life of the OA state alloy is the best, and both the UA state and the PA state have reached high cycle fatigue. After the alloy is aging heat treated, the grain size, recrystallization degree and microstructure that have a significant impact on fatigue performance are basically unchanged from before aging treatment. Therefore, the difference in fatigue performance in different aging states is mainly caused by the type and size of the precipitated phase during the aging process. Combined with Fig.10 (c) and Fig.10 (c) and (f) show that the precipitated phases of the OA alloy are mainly long strips of η' phase and η phase, and the size of the precipitated phase is large, the distribution range is more uniform, and the spacing between the precipitated phases is larger. The uncut η' metastable phase and η phase can hinder the slip of dislocations. From the UA state to the OA state, the expansion of the cuttable GP zone and η' phase, the evolution to the η phase, and the nucleation, growth and coarsening of the η phase are beneficial to improving the fatigue resistance of the alloy.

[0070] After the spray-formed 7055 aluminum alloy extruded rod was subjected to a single-stage aging treatment at 120℃ / 40h, it was found that the hardness of the alloy increased fastest in the first 2h of aging. As the aging time increased, the hardness of the alloy reached a peak hardness of 254.6HV after 10h aging. Then, the hardness gradually decreased with the continued increase of aging time, and finally stabilized. The yield strength and tensile strength of the alloy after the 120℃ single-stage aging treatment were significantly improved. The yield strength and tensile strength of the PA alloy were the best among the three states, which were 729MPa and 688MPa respectively. The elongation of the UA and OA alloys was close to and better than that of the PA alloy. The tensile fractures of the alloys in the three aging states all showed a mixed fracture mode of transgranular and intergranular.

[0071] After fatigue tests on alloys in three aging states, it was found that the fatigue life of the OA state alloy was the best at 222010 times. After aging heat treatment, the main precipitation phases in the UA state of 7055 aluminum alloy are a large number of fine GPⅡ zones that can be cut through. The precipitation phases in the PA state are mostly elliptical and elongated, fine and dispersed, mainly GPⅡ zones and a part of the η' phase that cannot be cut through. The precipitation phases in the OA state are obviously grown, mainly the η' metastable phase and η phase that cannot be cut through. The η' metastable phase and η phase that cannot be cut through can hinder the slip of dislocations, and the size of the precipitation phases is obviously grown. With the deepening of the aging degree, the precipitation phases in the matrix are obviously coarsened and grown, the size distribution of the precipitation phases is expanded, the average size increases, and the precipitation phases evolve from the GP zone and η' phase to the η' phase and η phase. With the deepening of the aging degree, the ability to resist fatigue cracks is improved.

[0072] In summary, after reading the present invention document, ordinary technicians in this field can make various other corresponding transformation schemes based on the technical scheme and technical concept of the present invention without creative mental work, which all fall within the scope of protection of the present invention.

Claims

1. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy, characterized in that: The following steps are involved: The aluminum alloy material is placed in a vacuum melting furnace to completely melt the aluminum alloy material and then kept warm to obtain liquid metal, and the liquid metal is sprayed with a spraying device to obtain a deposited alloy, and then heat-treated; Single-stage aging treatment of heat-treated aluminum alloys; Test the fatigue properties of aluminum alloys at multiple aging times; The precipitation phase of aluminum alloy with multiple aging times was detected.

2. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 1, characterized in that: The step of placing the alloy material into a vacuum furnace to completely melt the alloy material and then keeping the alloy material warm comprises: the alloy material is completely melted in a vacuum furnace at 820° C. to 880° C. and then keeping the alloy warm for 10 minutes.

3. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 2, characterized in that: The method of using a spray deposition device to prepare a deposited alloy from liquid metal includes: using a spray deposition device to prepare a columnar deposited alloy with a diameter of 180 mm and a height of 400 mm, selecting a columnar deposited alloy with a center diameter of 100 mm and a height of 200 mm for hot extrusion to obtain a rod alloy with a diameter of 40 mm.

4. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 3, characterized in that: The single-stage aging treatment of the heat-treated aluminum alloy includes a single-stage aging treatment of the rod alloy at 120°C.

5. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 4, characterized in that: The multiple aging conditions include an under-aging UA state, a peak-aging PA state and an over-aging OA state. The holding time of the under-aging UA state is 2 hours, the holding time of the peak-aging PA state is 10 hours, and the holding time of the over-aging OA state is 40 hours.

6. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 5, characterized in that: The fatigue performance of the aluminum alloy is tested, including: using a fatigue testing machine to perform a tension-compression fatigue test, with a stress level of 300 MPa, a frequency of 10 Hz, a stress ratio of R=0.1, a load type of sine wave, and the fatigue test is performed in an atmospheric environment at room temperature.

7. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 6, characterized in that: The fatigue performance testing of the aluminum alloy also includes: sampling fatigue specimens for fatigue performance testing of the aluminum alloy along the extrusion direction of the extruded rod, grinding and polishing the cross-section of the specimen of the extruded rod alloy with sandpaper, observing the specimen with a field emission scanning electron microscope at 20kV, and performing microstructural analysis and characterization on the extruded alloy.

8. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 7, characterized in that: The fatigue performance testing of the aluminum alloy also includes: placing multiple sample discs of the aluminum alloy in the aged state into an MT-PI type ion double-jet electrolytic thinning instrument to thin the samples, the electrolyte is 30% HNO3+70% CH3OH, the temperature of the thinning liquid is monitored and controlled at -30°C to -20°C by a thermometer, the current is controlled at 100-120mA, the voltage is 15-20V, and the microstructures of the aluminum alloys in the aged state are observed by a transmission electron microscope at 200kV.

9. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 8, characterized in that: The detection of the precipitation phase of the aluminum alloy at multiple aging times includes: using a transmission electron microscope to observe the TEM bright field image of the aluminum alloy at different aging times at 120° C.

10. A method for detecting single-stage aging precipitation phase and fatigue performance of aluminum alloy according to claim 9, characterized in that: The detection of the precipitation phase of the aluminum alloy at multiple aging times also includes: observing the SAED pattern of the crystal zone axis of the aluminum alloy at different aging times at 120° C. using a transmission electron microscope.